Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Vydyne® R433H BK0746 - PA66-GF33 - Ascend

Material Data Center offers the following functions for Vydyne® R433H BK0746:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vydyne datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Vydyne R433H BK0746 is designed to reinforce downgauged steel and aluminum used in vehicle body-in-white (BIW) structures, helping reduce weight without sacrificing safety or comfort.
R433H BK0746 has improved energy absorption over traditional glass-filled PA66, helping reduce noise, vibration and harshness (NVH) and absorbing impact energy from crashes. Using R433H BK0746 in the BIW structure reinforces sheet metal, helping manufacturers shave substantial weight and improve efficiency. Trends in lightweight and NVH are becoming even more paramount with the growth of Electric Vehicles. Vydyne R433H BK0746 has excellent performance attributes to support applications where this will be of prime importance such as battery frames and housings.
Caratteristiche Fisichesecco/condUnitáNorma del test
ISO Data
Ritiro di stampaggio, parallelo 0.6 / * % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.0 / * % ISO 294-4, 2577
Proprietà Meccanichesecco/condUnitáNorma del test
ISO Data
Modulo a trazione 9600 / 6200 MPa ISO 527
Carico unitario a trazione 150 / 103 MPa ISO 527
Deformazione a snervamento 3.3 / 7.4 % ISO 527
Modulo a flessione, 23°C 8400 / 6000 MPa ISO 178
Resistenza alla flessione 210 / 130 MPa ISO 178
Resistenza all'urto Charpy, +23°C 96 / 96 kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C 100 / 92 kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 24 / 27 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 17 / 16 kJ/m² ISO 179/1eA
Resistenza all'urto Izod con intaglio, +23°C 21 / 29 kJ/m² ISO 180/1A
Resistenza all'urto Izod con intaglio 15 / - kJ/m² ISO 180/1A
Temperatura -40 °C -
Proprietà Termichesecco/condUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 262 / * °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 245 / * °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 260 / * °C ISO 75-1/-2
Coeff.di dilatazione termica lin., parallelo 16 / * E-6/K ISO 11359-1/-2
Coeff.di dilatazione termica lin., perpend. 11 / * E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB / * class IEC 60695-11-10
Spessore provato 1.5 / * mm -
Reazione al fuoco a spessore h V-2 / * class IEC 60695-11-10
Spessore provato 0.4 / * mm -
ASTM Data
UL 94 combustibilitá V-2 - UL 94
Spessore testati 0.4 mm -
Proprietà Elettrichesecco/condUnitáNorma del test
ISO Data
Rigidità dielettrica 28 / - kV/mm IEC 60243-1
Altre Proprietàsecco/condUnitáNorma del test
Assorbimento d'acqua 1 / * % Sim. alla ISO 62
Assorbimento d'umidità 1.3 / * % Sim. alla ISO 62
Massa volumica 1350 / - kg/m³ ISO 1183
Raccomandazione de Processabilità Stampaggio ad IniezioneValoreUnitáNorma del test
Pre-essiccamento - Temperatura 80 °C -
Pre-essiccamento - Tempo 4 h -
Temperatura di fusione 285 - 305 °C -
Temperatura dello stampo 65 - 95 °C -
Zona 1 280 - 310 °C -
Zona 2 280 - 310 °C -
Zona 3 280 - 310 °C -
Temperatura dell ugello 280 - 310 °C -
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet, Nero
Additivi
Lubrificanti
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile al calore
Caratteristiche
Proprietà di barriera acustica
Resistenza Chimica
Resistenza chimica generale, Resistenza ai solventi, Resistenza all’olio
Applicazioni
Automotive, Incapsulamento
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.