Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Luran® S ECO 778T BC30 - ASA - INEOS Styrolution

Material Data Center offers the following functions for Luran® S ECO 778T BC30:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, CAE Interfaces

Check here, which other Luran datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Luran® S ECO 778T BC30 acrylonitrile styrene acrylate (ASA) polymer features high surface quality and good impact strength including enhanced colour fastness. The product delivers superior long-term performance when exposed to UV irradiation and additionally provide excellent chemical resistance. Luran® S ECO 778T BC30 is an injection molding grade with enhanced heat resistance and best chemical resistance among the Luran® S grades. Luran® S ECO 778T BC30 is an ISCC compliant product leading to a substitution of fossil source styrene with ISCC certified bio-attributed styrene.
Carbon Footprint Reduction vs Fossil-Based (3rd party validated): 39 % (ISO 14044)
Attributed Content of ISCC-certified Bio-Circular Sources (min.): 30 %
Caratteristiche FisicheValoreUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 5 cm³/10min ISO 1133
Temperatura 220 °C -
Carico 10 kg -
Ritiro di stampaggio, parallelo 0.6 % ISO 294-4, 2577
Densità del fuso 960 kg/m³ -
Conduttività termica del fuso 0.185 W/(m K) -
Capacità termica specifica del fuso 2160 J/(kg K) -
Temperatura di estrazione 98 °C -
Proprietà MeccanicheValoreUnitáNorma del test
ISO Data
Modulo a trazione 2500 MPa ISO 527
Carico unitario a trazione 54 MPa ISO 527
Deformazione a snervamento 3.4 % ISO 527
Deformazione nominale a rottura 8 % ISO 527
Modulo a flessione, 23°C 2450 MPa ISO 178
Resistenza alla flessione 80 MPa ISO 178
Resistenza all'urto Charpy, +23°C 220 kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 15 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 4 kJ/m² ISO 179/1eA
Ball indentation hardness 85 MPa ISO 2039-1
Proprietà TermicheValoreUnitáNorma del test
ISO Data
Temp.di inflessione sotto carico, 1.80 MPa 103 °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 106 °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 104 °C ISO 306
Coeff.di dilatazione termica lin., parallelo 95 E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB class IEC 60695-11-10
Spessore provato 1.5 mm -
Yellow Card disponibile - -
Reazione al fuoco a spessore h HB class IEC 60695-11-10
Spessore provato 3.0 mm -
Yellow Card disponibile - -
Velocità di avanzamento fiamma, FMVSS, spessore 1mm 30[1] mm/min ISO 3795 (FMVSS 302)
Other Standards[S]
Conduttività termica, stato solido 0.17 W/(m K) DIN 52612-1
1: 2 mm  S: These properties are reported by the producer according standards that are different to our defaults.
Altre ProprietàValoreUnitáNorma del test
Assorbimento d'acqua 1.65 % Sim. alla ISO 62
Assorbimento d'umidità 0.35 % Sim. alla ISO 62
Massa volumica 1070 kg/m³ ISO 1183
Bulk density 600 kg/m³ -
Raccomandazione de Processabilità Stampaggio ad IniezioneValoreUnitáNorma del test
Pre-essiccamento - Temperatura 80 °C -
Pre-essiccamento - Tempo 2 - 4 h -
Temperatura di fusione 240 - 280 °C -
Temperatura dello stampo 40 - 80 °C -
Funzioni
Viscosità-Velocità di taglio , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Sforzo di taglio-Velocità di taglio , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Modulo dinamico a taglio-temperatura , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Sforzi-deformazione , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Modulo secante-deformazione , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Sforzi-deformazioni (isocrona) 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Modulo di scorrimento-tempo 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Curva di scorrimento 23°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Sforzi-deformazioni (isocrona) 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Modulo di scorrimento-tempo 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Curva di scorrimento 60°C, Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Volume specifico-temperatura (pvT) , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Modulo a taglio-temperatura , Luran® S ECO 778T BC30, ASA, INEOS Styrolution
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Additivi
Agente di distacco
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile alla luce, Estab. agli U.V. o per applicaz.in esterni, Stabilizzato o stabile al calore
Resistenza Chimica
Resistenza chimica generale
Certifications
Contiene risorse rinnovabili, ISCC Plus
Applicazioni
Automotive, Elettrotecnica ed electrici, Attrezzature sportive, Giocattoli
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Altre informazioni
Stampaggio ad Iniezione
PREPROCESSING

Pre-drying, Temperature: 80°C

Pre-drying, Time: 2 - 4h

PROCESSING

Melt temperature, range: 240 - 280°C

Mold temperature, range: 40 - 80°C

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com