Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Promyde® B30 P2 HI60 - PA6 - Nurel S.A.
Material Data Center offers the following functions for Promyde® B30 P2 HI60:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces
Check here, which other Promyde datasheets, application examples or technical articles are available in Material Data Center
Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our
disclaimer.
Caratteristiche Fisiche | secco/cond | Unitá | Norma del test |
ISO Data |
Indice di fusione di volume, MVR |
120 / * |
cm³/10min |
ISO 1133 |
Temperatura |
275 / * |
°C |
- |
Carico |
5 / * |
kg |
- |
Ritiro di stampaggio, parallelo |
0.8 / * |
% |
ISO 294-4, 2577 |
Ritiro di stampaggio, perpendicolare |
0.8 / * |
% |
ISO 294-4, 2577 |
Proprietà Meccaniche | secco/cond | Unitá | Norma del test |
ISO Data |
Modulo a trazione |
2100 / 1300 |
MPa |
ISO 527 |
Resistenza a trazione |
60 / 35 |
MPa |
ISO 527 |
Deformazione a snervamento |
4.5 / 35 |
% |
ISO 527 |
Deformazione a rottura |
35 / >50 |
% |
ISO 527 |
Modulo a flessione, 23°C |
1700 / 900 |
MPa |
ISO 178 |
Resistenza alla flessione |
70 / 35 |
MPa |
ISO 178 |
Resistenza all'urto Charpy, +23°C |
N / N |
kJ/m² |
ISO 179/1eU |
Resistenza all'urto Charpy, -30°C |
N / - |
kJ/m² |
ISO 179/1eU |
Resist. urto Charpy con intaglio, +23°C |
65 / 125 |
kJ/m² |
ISO 179/1eA |
Resist. urto Charpy con intaglio, -30°C |
20 / - |
kJ/m² |
ISO 179/1eA |
Proprietà Termiche | secco/cond | Unitá | Norma del test |
ISO Data |
Temperatura di fusione, 10°C/min |
222 / * |
°C |
ISO 11357-1/-3 |
Temp.di inflessione sotto carico, 1.80 MPa |
50 / * |
°C |
ISO 75-1/-2 |
Coeff.di dilatazione termica lin., parallelo |
120 / * |
E-6/K |
ISO 11359-1/-2 |
Coeff.di dilatazione termica lin. , perpend. |
120 / * |
E-6/K |
ISO 11359-1/-2 |
Reaz. al fuoco spess.nom. 1.5mm |
HB / * |
class |
IEC 60695-11-10 |
Spessore provato |
1.5 / * |
mm |
- |
Proprietà Elettriche | secco/cond | Unitá | Norma del test |
ISO Data |
Res. Alle correnti striscianti superficiali |
600 / - |
- |
IEC 60112 |
Other Standards[S] |
Costante dielettrica relativa, 1MHz |
2.7 / 4 |
- |
IEC 60250 |
Fattore di dissipazione, 1MHz |
160 / 1000 |
E-4 |
IEC 60250 |
Resistività volumica |
1E13 / 1E11 |
Ohm*m |
IEC 60093 |
S: | These properties are reported by the producer according standards that are different to our defaults. |
Altre Proprietà | secco/cond | Unitá | Norma del test |
Assorbimento d'acqua |
8.1 / * |
% |
Sim. alla ISO 62 |
Assorbimento d'umidità |
2.6 / * |
% |
Sim. alla ISO 62 |
Massa volumica |
1100 / - |
kg/m³ |
ISO 1183 |
Proprietà Specifiche Materiale | secco/cond | Unitá | Norma del test |
ISO Data |
Numero di viscosità |
125 / * |
cm³/g |
ISO 307, 1157, 1628 |
Raccomandazione de Processabilità Stampaggio ad Iniezione | Valore | Unitá | Norma del test |
Pre-essiccamento - Temperatura |
<80 |
°C |
- |
Pre-essiccamento - Tempo |
4 - 6 |
h |
- |
Temperatura di fusione |
250 - 270 |
°C |
- |
Temperatura dello stampo |
40 - 80 |
°C |
- |
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Additivi
Agente di distacco
Caratteristiche speciali
Alto urto o modificato all'urto, Stabilizzato o stabile al calore
Disponibilità geografica
Europa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com
Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.
Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.