Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® N2720 M210 AT - POM-MD10 - BASF

Material Data Center offers the following functions for Ultraform® N2720 M210 AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Grade with enhanced stiffness and strength as well as good wear properties, e.g. used for conveyor belts and transportation systems.

Abbreviated designation according to ISO 1043: POM-MD
Designation according to ISO 29988-POM-K,MD,M-GNRS2,3-2
Caratteristiche FisicheValoreUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 7 cm³/10min ISO 1133
Temperatura 190 °C -
Carico 2.16 kg -
Ritiro di stampaggio, parallelo 1.7 % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.9 % ISO 294-4, 2577
Proprietà MeccanicheValoreUnitáNorma del test
ISO Data
Modulo a trazione 3800 MPa ISO 527
Carico unitario a trazione 63 MPa ISO 527
Deformazione a snervamento 9.5 % ISO 527
Deformazione nominale a rottura 18 % ISO 527
Resistenza all'urto Charpy, +23°C 90 kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C 90 kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 3.5 kJ/m² ISO 179/1eA
Resistenzia all'urto Charpy con intaglio, -30°C 3.5 kJ/m² ISO 179/1eA
Proprietà TermicheValoreUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 166 °C ISO 11357-1/-3
Temp.di inflessione sotto carico, 1.80 MPa 115 °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 150 °C ISO 306
Coeff.di dilatazione termica lin., parallelo 80 E-6/K ISO 11359-1/-2
Reaz. al fuoco spess.nom. 1.5mm HB class IEC 60695-11-10
Spessore provato 1.6 mm -
Yellow Card disponibile - -
Reazione al fuoco a spessore h HB class IEC 60695-11-10
Spessore provato 3.2 mm -
Yellow Card disponibile - -
Proprietà ElettricheValoreUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 3.9 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 3.8 - IEC 62631-2-1
Fattore di dissipazione, 100Hz 50 E-4 IEC 62631-2-1
Fattore di dissipazione, 1MHz 60 E-4 IEC 62631-2-1
Resistività volumica 1E10 Ohm*m IEC 62631-3-1
Resistività superficiale 1E14 Ohm IEC 62631-3-2
Rigidità dielettrica 40 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali 600 - IEC 60112
Altre ProprietàValoreUnitáNorma del test
Assorbimento d'acqua 0.8 % Sim. alla ISO 62
Assorbimento d'umidità 0.2 % Sim. alla ISO 62
Massa volumica 1490 kg/m³ ISO 1183
Funzioni
Sforzi-deformazione , Ultraform® N2720 M210 AT, POM-MD10, BASF
Modulo secante-deformazione , Ultraform® N2720 M210 AT, POM-MD10, BASF
Sforzi-deformazioni (isocrona) 23°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Modulo di scorrimento-tempo 23°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Curva di scorrimento 23°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Sforzi-deformazioni (isocrona) 60°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Modulo di scorrimento-tempo 60°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Curva di scorrimento 60°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Sforzi-deformazioni (isocrona) 120°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Modulo di scorrimento-tempo 120°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Curva di scorrimento 120°C, Ultraform® N2720 M210 AT, POM-MD10, BASF
Modulo a taglio-temperatura , Ultraform® N2720 M210 AT, POM-MD10, BASF
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Additivi
Lubrificanti
Caratteristiche
Copolimero
Disponibilità geografica
Altre informazioni
Stampaggio ad Iniezione
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min

Processing

Usual single-flighted three-section screws with an effective screw length of at least 15 D, better 20 - 23 D are suitable for the injection molding of Ultraform.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.


Postprocessing

If parts were produced at a comparatively low mold temperature (e.g. in order to obtain short cycle times) and must not change their geometry in use thermal postprocessing inducing dimensional changes by postcrystallization may be necessary. In such cases parts should be stored in an oven with recirculated air at temperatures of 100 - 130 °C until dimensions don't change significantly any further. The time needed for this has to be determined experimentally.
Resistenza chimica
Acidi
Acido acetico (5% da massa) (23°C)
Acido lattico (10% da massa) (23°C)
Acido cloridrico (36% da massa) (23°C)
Acido nitrico (40% da massa) (23°C)
Acido solforico (38% da massa) (23°C)
Acido solforico (5% da massa) (23°C)
Soluzione acida cromica (40% da massa) (23°C)
Basi
Soluzione dell' idrossido del sodio (35% da massa) (23°C)
Soluzione dell' idrossido del sodio (1% da massa) (23°C)
Soluzione dell' idrossido di ammonio (10% da massa) (23°C)
Alcool
Alcool di isopropile (23°C)
Metanolo (23°C)
Etanolo (23°C)
Idrocarburi
n-Hexane (23°C)
Toluene (23°C)
isoottano (23°C)
Chetoni
Acetone (23°C)
Eteri
Etere Etilico (23°C)
Oli minerali
Olio multigrade del motore di SAE 10W40 (130°C)
Olio dell' ipoide-ingranaggio di SAE 80/90 (130°C)
Combustibili Standard
Liquido 1 di ISO 1817 (60°C)
Liquido 2 di ISO 1817 (60°C)
Liquido 3 di ISO 1817 (60°C)
Liquido 4 di ISO 1817 (60°C)
Combust. stand. senza alcool (pref. ISO 1817 liquido C) (23°C)
Combust. stand. con alcool (pref. ISO 1817 liquido 4) (23°C)
Combustibile diesel (pref. ISO 1817 liquido F) (23°C)
Combustibile diesel (pref. ISO 1817 liquido F) (>90°C)
Soluzioni saline
Soluzione del cloruro di sodio (10% da massa) (23°C)
Soluzione dell' ipoclorito del sodio (10% da massa) (23°C)
Soluzione del carbonato di sodio (20% da massa) (23°C)
Soluzione del carbonato di sodio (2% da massa) (23°C)
Altri
Acetato etilico (23°C)
Perossido di idrogeno (23°C)
Liquido di freno del DOT N° 4 (130°C)
Glicol etilenico (50% da massa) in acqua (108°C)
acido oleico 50% + olio di oliva 50% (23°C)
Acqua (23°C)
Acqua deionizzata (90°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com