Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® 2000 G - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® 2000 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Testo del prodotto
Medium viscosity, unreinforced polyether ether ketone

VESTAKEEP® 2000 G is a medium viscosity, unreinforced polyether ether ketone for injection molding.

The semi-crystalline polymer features superior, thermal and chemical resistance. Parts made from VESTAKEEP® 2000 G are of low flammability.

VESTAKEEP® 2000 G can be processed on common injection molding machines for thermoplastics.

We recommend a melt temperature between 360°C and 380°C during the injection molding process. The mold temperature should be within a range of 160°C to 200°C, preferably 180°C.

VESTAKEEP® 2000 G is supplied as granules in 25 kg boxes with moisture-proof polyethylene inliners.

Pigmentation may affect values.

For information about processing VESTAKEEP® 2000 G, please follow the general recommendations in our brochure "VESTAKEEP® PEEK Processing Guidelines“.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT  WWW.INDUSTRIAL.VESTAKEEP.COM
Caratteristiche FisicheValoreUnitáNorma del test
ISO Data
Indice di fusione di volume, MVR 70 cm³/10min ISO 1133
Temperatura 380 °C -
Carico 5 kg -
Ritiro di stampaggio, parallelo 1.1 % ISO 294-4, 2577
Ritiro di stampaggio, perpendicolare 1.1 % ISO 294-4, 2577
Proprietà MeccanicheValoreUnitáNorma del test
ISO Data
Modulo a trazione 3700 MPa ISO 527
Carico unitario a trazione 100 MPa ISO 527
Deformazione a snervamento 5 % ISO 527
Deformazione nominale a rottura 20 % ISO 527
Resistenza all'urto Charpy, +23°C N kJ/m² ISO 179/1eU
Resistenza all'urto Charpy, -30°C N kJ/m² ISO 179/1eU
Resistenzia all'urto Charpy con intaglio, +23°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
Resistenzia all'urto Charpy con intaglio, -30°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
Proprietà TermicheValoreUnitáNorma del test
ISO Data
Temperatura di fusione, 10°C/min 340 °C ISO 11357-1/-3
Temperatura di transizione vetrosa, 10°C/min 150 °C ISO 11357-1/-2
Temp.di inflessione sotto carico, 1.80 MPa 155 °C ISO 75-1/-2
Temp.di inflessione sotto carico, 0.45 MPa 205 °C ISO 75-1/-2
Temp.di rammollimento Vicat, B 310 °C ISO 306
Coeff.di dilatazione termica lin., parallelo 60 E-6/K ISO 11359-1/-2
Yellow Card disponibile - -
Indice di ossigeno 38 % ISO 4589-1/-2
Proprietà ElettricheValoreUnitáNorma del test
ISO Data
Costante dielettrica relativa, 100Hz 2.8 - IEC 62631-2-1
Costante dielettrica relativa, 1MHz 2.8 - IEC 62631-2-1
Fattore di dissipazione, 1MHz 50 E-4 IEC 62631-2-1
Resistività volumica >1E13 Ohm*m IEC 62631-3-1
Resistività superficiale 1E15 Ohm IEC 62631-3-2
Rigidità dielettrica 32.6 kV/mm IEC 60243-1
Res. Alle correnti striscianti superficiali 200 - IEC 60112
Altre ProprietàValoreUnitáNorma del test
Assorbimento d'acqua 0.5 % Sim. alla ISO 62
Assorbimento d'umidità 0.12 % Sim. alla ISO 62
Massa volumica 1300 kg/m³ ISO 1183
Funzioni
Sforzi-deformazioni (isocrona) 150°C, VESTAKEEP® 2000 G, PEEK, Evonik
Modulo di scorrimento-tempo 150°C, VESTAKEEP® 2000 G, PEEK, Evonik
Curva di scorrimento 150°C, VESTAKEEP® 2000 G, PEEK, Evonik
Modulo a taglio-temperatura , VESTAKEEP® 2000 G, PEEK, Evonik
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione, Estrusione Film, Altre Estrusioni
Forma fisica disponibile
Pellet
Caratteristiche speciali
Stabilizzato o stabile al calore
Disponibilità geografica
Nord America, Europa, Asia Oceano Pacifico, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.