Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Apec® 1745 RE - PC - Covestro Deutschland AG

Material Data Center offers the following functions for Apec® 1745 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Apec datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
  • MVR (330°C/2.16kg) 17 cm³/10 min
  • easy release
  • for superheated steam sterilization up to 143 °C
  • meets criteria of US Pharmacopeia (USP) Class VI
  • biocompatible according to many ISO 10993-1 test requirements
  • softening temperature (VST/B 120)=170 °C
  • Films for medical packaging
  • Contact lens holders
  • Medical vessels
  • Safety valve for respiration aids
  • Syringe tops
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 17 cm³/10min ISO 1133
温度 330 °C -
荷重 2.16 kg -
メルトフローレート, MFI 17 g/10min ISO 1133
温度 330 °C -
荷重 2.16 kg -
成形収縮率, 平行 0.8 % ISO 294-4, 2577
成形収縮率, 直角 0.8 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 2400 MPa ISO 527
降伏応力 70 MPa ISO 527
降伏ひずみ 6.8 % ISO 527
破壊呼びひずみ >50 % ISO 527
曲げ弾性率, 23°C 2400 MPa ISO 178
シャルピー衝撃強さ, +23°C N kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C N kJ/m² ISO 179/1eU
Ball indentation hardness 120 MPa ISO 2039-1
熱的特性単位テスト基準
ISO データ
荷重たわみ温度, 1.80 MPa 148 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 161 °C ISO 75-1/-2
ビカット軟化温度, B 170 °C ISO 306
線膨張係数, 平行 65 E-6/K ISO 11359-1/-2
線膨張係数, 直角 65 E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 1.5 mm -
Yellow Card 可用 はい - -
酸素指数 25 % ISO 4589-1/-2
グローワイヤ燃焼性指数 (GWFI) 850 °C IEC 60695-2-12
GWFI - 試験片の厚さ 2 mm -
電気的特性.単位テスト基準
ISO データ
比誘電率, 100Hz 3 - IEC 62631-2-1
比誘電率, 1MHz 2.9 - IEC 62631-2-1
誘電正接, 100Hz 10 E-4 IEC 62631-2-1
誘電正接, 1MHz 80 E-4 IEC 62631-2-1
体積抵抗率 >1E13 Ohm*m IEC 62631-3-1
表面抵抗率 >1E15 Ohm IEC 62631-3-2
耐電圧 35 kV/mm IEC 60243-1
耐トラッキング性 250 - IEC 60112
光学特性単位テスト基準
ISO Data
視感透過率 88[1] % ISO 13468-1, -2
Other Standards[S]
くっせつりつ 1.58 - ISO 489
1: Clear transparent materials  S: These properties are reported by the producer according standards that are different to our defaults.
その他の特性.単位テスト基準
吸水率 0.3 % Sim. to ISO 62
吸湿率 0.12 % Sim. to ISO 62
密度 1170 kg/m³ ISO 1183
試験片の成形条件.単位テスト基準
ISO データ
射出成形, 樹脂温度 330 °C ISO 294
射出成形, 金型温度 100 °C ISO 294
射出成形, 射出速度 200 mm/s ISO 294
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 130 °C -
Pre-drying - Time 2 - 3 h -
Processing humidity ≤0.02 % -
樹脂温度 320 - 340 °C -
金型温度 110 - 130 °C -
Zone 1 290 - 300 °C -
Zone 2 300 - 310 °C -
Zone 3 310 - 320 °C -
Nozzle temperature 320 - 330 °C -
Back pressure 5 - 15 MPa -
特殊な特性
成形加工法.
射出成形.
添加剤.
離型剤.
特殊な特性.
熱安定化., 透明., 滅菌可能, 蒸気滅菌
Certifications
Contains renewable resources, Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved, ISCC Plus
アプリケーション
医療の, パッケージング
領域別の利用可能性
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.