Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of FORTRON® 4665B6 - PPS-(MD+GF)65 - Celanese

Material Data Center offers the following functions for FORTRON® 4665B6:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Fortron datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Fortron 4665B6 offers a high Comparative Tracking Index (CTI) for application requiring resistance to high voltage. The product exhibits good heat and chemical resistance as well as good electrical properties. This grade is also inherently flame-retardant. Due to the balance of mineral and glass fibers the warpage is very low. Applications include electronic components (i.e. lamp sockets, housings and position frames).

Flammability @1.6mm nom. thickn.V-0-
Flammability at thickness h (0.82 mm)V-0-
Processing/Physical Characteristics単位テスト基準
ISO データ
成形収縮率, 平行 0.2 % ISO 294-4, 2577
成形収縮率, 直角 0.6 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 17300 MPa ISO 527
破壊応力 110 MPa ISO 527
破壊ひずみ 1.2 % ISO 527
シャルピー衝撃強さ, +23°C 18 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 18 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 6 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 6 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 280 °C ISO 11357-1/-3
ガラス転移点, 10°C/min 90 °C ISO 11357-1/-2
荷重たわみ温度, 1.80 MPa 270 °C ISO 75-1/-2
荷重たわみ温度, 8.00 MPa 215 °C ISO 75-1/-2
線膨張係数, 平行 20 E-6/K ISO 11359-1/-2
線膨張係数, 直角 25 E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 V-0 class IEC 60695-11-10
試験片の厚さ 1.5 mm -
厚さhでの燃焼性 V-0 class IEC 60695-11-10
試験片の厚さ 0.8 mm -
電気的特性.単位テスト基準
ISO データ
比誘電率, 1MHz 5.3 - IEC 62631-2-1
誘電正接, 1MHz 20 E-4 IEC 62631-2-1
体積抵抗率 >1E13 Ohm*m IEC 62631-3-1
表面抵抗率 >1E15 Ohm IEC 62631-3-2
耐電圧 25 kV/mm IEC 60243-1
その他の特性.単位テスト基準
吸水率 0.02 % Sim. to ISO 62
密度 2030 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 130 - 140 °C -
Pre-drying - Time 3 - 4 h -
樹脂温度 320 - 340 °C -
金型温度 ≥140 °C -
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット.
添加剤.
離型剤.
特殊な特性.
難燃., 熱安定化.
な特性
Low Warpage
耐薬品性
General Chemical Resistance
アプリケーション
電気電子
領域別の利用可能性
北アメリカ., ヨーロッパ., 南・中央アメリカ., 近東/アフリカ
その他の情報
村遜速揃
Predrying in a dehumidified air dryer at 130 - 140 degC/3-4 hours is recommended.
On injection molding machines with 15-25 D long three-section screws, as are usual in the trade, the FORTRON is processable. A shut-off nozzle is preferred to a free-flow nozzle.

Melt temperature 320-340 degC
Mold wall temperature at least 140 degC

A medium injection rate is normally preferred. All mold cavities must be effectively vented.
Tool temperature of at least 135 degC is recommended for parts to achieve maximum crystallizable potential.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.