Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of HOSTAFORM® C 2521 G - POM - Celanese

Material Data Center offers the following functions for HOSTAFORM® C 2521 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Hostaform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 1.5 cm³/10min ISO 1133
温度 190 °C -
荷重 2.16 kg -
機械的特性単位テスト基準
ISO データ
引張弾性率 2100 MPa ISO 527
降伏応力 44 MPa ISO 527
降伏ひずみ 12 % ISO 527
破壊呼びひずみ 15 % ISO 527
シャルピー衝撃強さ, +23°C 50 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 50 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 5 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 4.5 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 165 °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 84 °C ISO 75-1/-2
線膨張係数, 平行 100 E-6/K ISO 11359-1/-2
電気的特性.単位テスト基準
ISO データ
比誘電率, 100Hz 3.8 - IEC 62631-2-1
比誘電率, 1MHz 3.8 - IEC 62631-2-1
誘電正接, 100Hz 20 E-4 IEC 62631-2-1
誘電正接, 1MHz 70 E-4 IEC 62631-2-1
体積抵抗率 1E12 Ohm*m IEC 62631-3-1
表面抵抗率 1E14 Ohm IEC 62631-3-2
耐電圧 35 kV/mm IEC 60243-1
その他の特性.単位テスト基準
吸水率 0.8 % Sim. to ISO 62
吸湿率 0.2 % Sim. to ISO 62
密度 1340 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 100 - 120 °C -
Pre-drying - Time 3 - 6 h -
Processing humidity ≤0.2 % -
樹脂温度 190 - 210 °C -
金型温度 80 - 120 °C -
機能
 応力-ひずみ. , HOSTAFORM® C 2521 G, POM, Celanese
 割線弾性率−ひずみ. , HOSTAFORM® C 2521 G, POM, Celanese
特殊な特性
成形加工法.
射出成形., フィルム押出成形., 異形押出成形., シート押出成形., その他の押出成形., ブロー成形.
納入形状.
ペレット.
添加剤.
滑剤., 離型剤.
な特性
Thermal Stability, Copolymer
耐薬品性
Alkali Resistance, Solvent Resistance, Hydrolytically Stable, Oxidation Resistance
アプリケーション
自動車
領域別の利用可能性
北アメリカ., ヨーロッパ.
その他の情報
村遜速揃
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %
Standard injection moulding machines with three phase (15 to 25 D)
plasticating screws will fit.

Conditioning e.g. moisturizing is not necessary.
フィルム押出成形.
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
その他の押出成形.
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
族臓遜造揃
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
促揃臓村促速揃
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.