Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of HOSTAFORM® C 52021 - POM - Celanese

Material Data Center offers the following functions for HOSTAFORM® C 52021:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Hostaform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Chemical abbreviation according to ISO 1043-1: POM Molding compound ISO 29988- POM-K, M-GNR, 06-002 POM copolymer Extremely easy flowing Injection molding type for very thin-walled precision molded parts with unfavourite flow-path-wallthickness relation; permits processing at reduced temperature and also shorter cycle times; for mechanical lower requirements; good chemical resistance to solvents, fuel and strong alkalis as well as good hydrolysis resistance; high resistance to thermal and oxidative degradation. Monomers and additives are listed in EU-Regulation (EU) 10/2011 FDA compliant according to 21 CFR 177.2470 UL-registration in natural a thickness more than 0.81 mm, in black a thickness more than 1.5 mm as UL 94 HB, temperature index UL 746 B for a thickness of 1.5 mm, electrical 105 °C, mechanical 90 °C Burning rate ISO 3795 and FMVSS 302 < 75 mm/min for a thickness more than 1 mm. Ranges of applications: For very thin-walled precision molded parts with unfavourite flow-path-wallthickness relation; permits processing at reduced temperature and also shorter cycle times. FDA = Food and Drug Administration (USA) FMVSS = Federal Motor Vehicle Safety Standard (USA) UL = Underwriters Laboratories (USA)

Flammability @1.6mm nom. thickn.HB-
Flammability at thickness h (0.81 mm)HBUL recognition (h)
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 39 cm³/10min ISO 1133
温度 190 °C -
荷重 2.16 kg -
成形収縮率, 平行 1.9 % ISO 294-4, 2577
成形収縮率, 直角 1.8 % ISO 294-4, 2577
溶融時の密度 1200 kg/m³ -
溶融時の熱伝導率 0.155 W/(m K) -
溶融時の比熱 2060 J/(kg K) -
突き出し時の時の温度 140 °C -
機械的特性単位テスト基準
ISO データ
引張弾性率 3000 MPa ISO 527
降伏応力 65 MPa ISO 527
降伏ひずみ 7 % ISO 527
破壊呼びひずみ 15 % ISO 527
シャルピー衝撃強さ, +23°C 150 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 150 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 5 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 5 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 166 °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 106 °C ISO 75-1/-2
線膨張係数, 平行 110 E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 1.5 mm -
厚さhでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 0.8 mm -
Yellow Card 可用 はい - -
電気的特性.単位テスト基準
ISO データ
比誘電率, 100Hz 4 - IEC 62631-2-1
比誘電率, 1MHz 4 - IEC 62631-2-1
誘電正接, 100Hz 30 E-4 IEC 62631-2-1
誘電正接, 1MHz 50 E-4 IEC 62631-2-1
体積抵抗率 1E12 Ohm*m IEC 62631-3-1
表面抵抗率 1E14 Ohm IEC 62631-3-2
耐電圧 35 kV/mm IEC 60243-1
その他の特性.単位テスト基準
吸水率 0.65 % Sim. to ISO 62
吸湿率 0.2 % Sim. to ISO 62
密度 1410 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 100 - 120 °C -
Pre-drying - Time 3 - 6 h -
Processing humidity ≤0.2 % -
樹脂温度 190 - 210 °C -
金型温度 80 - 120 °C -
機能
 粘度せん断速度. , HOSTAFORM® C 52021, POM, Celanese
 せん断応力-せん断速度. , HOSTAFORM® C 52021, POM, Celanese
 せん断弾性率-温度. , HOSTAFORM® C 52021, POM, Celanese
 応力-ひずみ. , HOSTAFORM® C 52021, POM, Celanese
 割線弾性率−ひずみ. , HOSTAFORM® C 52021, POM, Celanese
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット., 黒, ナチュラルカラー
添加剤.
離型剤.
な特性
Thermal Stability, Copolymer
耐薬品性
Alkali Resistance, Solvent Resistance, Hydrolytically Stable, Oxidation Resistance
Certifications
Food contact, Food approval 10/2011, Food approval FDA 21 CFR, Drinking water contact
アプリケーション
自動車
領域別の利用可能性
北アメリカ., ヨーロッパ., アジア/太平洋地域., 南・中央アメリカ., 近東/アフリカ
その他の情報
村遜速揃
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %
Standard injection moulding machines with three phase (15 to 25 D)
plasticating screws will fit.

Conditioning e.g. moisturizing is not necessary.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.