Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Makroblend® M4000 FR - (PC+PBT) FR(16) - Covestro Deutschland AG

Material Data Center offers the following functions for Makroblend® M4000 FR:
unit conversion, PDF datasheet print, comparison with other plastics, application examples, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Makroblend datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
  • (PC+PBT) Blend, injection molding grade, flame retardant, excellent chemical resistance. Manufactured according to GMP, tested only according to ISO 10993-5 and ISO 10993-10 for contact with uncompromised skin only
  • for questions regarding biocompatibility we ask for an email inquiry under plastics@covestro.com. Limited colorability: recommended for whites and light colors only.
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 18 cm³/10min ISO 1133
温度 260 °C -
荷重 5 kg -
成形収縮率, 平行 0.8 % ISO 294-4, 2577
成形収縮率, 直角 0.8 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 2300 MPa ISO 527
降伏応力 56 MPa ISO 527
降伏ひずみ 4.3 % ISO 527
破壊呼びひずみ >50 % ISO 527
曲げ弾性率, 23°C 2300 MPa ISO 178
曲げ強さ 86 MPa ISO 178
ノッチ付きIzod衝撃強さ, +23°C 40 kJ/m² ISO 180/1A
ノッチ付きIzod衝撃強さ 12 kJ/m² ISO 180/1A
温度 -30 °C -
Ball indentation hardness 117 MPa ISO 2039-1
熱的特性単位テスト基準
ISO データ
荷重たわみ温度, 1.80 MPa 85 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 115 °C ISO 75-1/-2
ビカット軟化温度, B 130 °C ISO 306
線膨張係数, 平行 80 E-6/K ISO 11359-1/-2
線膨張係数, 直角 80 E-6/K ISO 11359-1/-2
厚さhでの燃焼性 V-0 class IEC 60695-11-10
試験片の厚さ 2.0 mm -
Yellow Card 可用 はい - -
厚さhでの燃焼性 5V 5VA class IEC 60695-11-20
試験片の厚さ 3.0 mm -
Yellow Card 可用 はい - -
電気的特性.単位テスト基準
ISO データ
比誘電率, 100Hz 3.4 - IEC 62631-2-1
比誘電率, 1MHz 3.2 - IEC 62631-2-1
誘電正接, 100Hz 20 E-4 IEC 62631-2-1
誘電正接, 1MHz 200 E-4 IEC 62631-2-1
体積抵抗率 >1E13 Ohm*m IEC 62631-3-1
表面抵抗率 1E15 Ohm IEC 62631-3-2
耐電圧 46 kV/mm IEC 60243-1
耐トラッキング性 225 - IEC 60112
その他の特性.単位テスト基準
吸水率 0.4 % Sim. to ISO 62
吸湿率 0.12 % Sim. to ISO 62
密度 1340 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 110 °C -
Pre-drying - Time 2 - 4 h -
Processing humidity ≤0.01 % -
樹脂温度 250 - 270 °C -
金型温度 60 - 100 °C -
Zone 1 245 - 255 °C -
Zone 2 250 - 260 °C -
Zone 3 255 - 265 °C -
Nozzle temperature 255 - 270 °C -
Back pressure 5 - 15 MPa -
特殊な特性
成形加工法.
射出成形.
特殊な特性.
難燃.
耐薬品性
General Chemical Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993
アプリケーション
医療の
領域別の利用可能性
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.