Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® H4320 AT - POM - BASF

Material Data Center offers the following functions for Ultraform® H4320 AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
High-molecular-weight grade for the extrusion of semifinished product; particularly thick walled product can be extruded at high output rates; the material also features high thermal stability and low discoloration.

Abbreviated designation according to ISO 1043-1: POM
Designation according to ISO 29988-POM-K,,E-GNR,1-2
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 2.2 cm³/10min ISO 1133
温度 190 °C -
荷重 2.16 kg -
成形収縮率, 平行 2.2 % ISO 294-4, 2577
成形収縮率, 直角 2.1 % ISO 294-4, 2577
突き出し時の時の温度 110 °C -
機械的特性単位テスト基準
ISO データ
引張弾性率 2400 MPa ISO 527
降伏応力 60 MPa ISO 527
降伏ひずみ 11 % ISO 527
破壊呼びひずみ 31 % ISO 527
引張クリープ弾性率, 1h 1800 MPa ISO 899-1
引張クリープ弾性率, 1000h 1300 MPa ISO 899-1
シャルピー衝撃強さ, +23°C 280 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 250 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 6.5 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 5.5 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 163 °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 90 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 155 °C ISO 75-1/-2
ビカット軟化温度, B 150 °C ISO 306
線膨張係数, 平行 120 E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 1.6 mm -
Yellow Card 可用 はい - -
厚さhでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 0.8 mm -
Yellow Card 可用 はい - -
酸素指数 15 % ISO 4589-1/-2
電気的特性.単位テスト基準
ISO データ
比誘電率, 100Hz 3.8 - IEC 62631-2-1
比誘電率, 1MHz 3.8 - IEC 62631-2-1
誘電正接, 100Hz 10 E-4 IEC 62631-2-1
誘電正接, 1MHz 50 E-4 IEC 62631-2-1
体積抵抗率 1E11 Ohm*m IEC 62631-3-1
表面抵抗率 1E13 Ohm IEC 62631-3-2
耐電圧 40 kV/mm IEC 60243-1
耐トラッキング性 600 - IEC 60112
その他の特性.単位テスト基準
吸水率 1 % Sim. to ISO 62
吸湿率 0.25 % Sim. to ISO 62
密度 1400 kg/m³ ISO 1183
試験片の成形条件.単位テスト基準
ISO データ
射出成形, 樹脂温度 200 °C ISO 294
射出成形, 金型温度 90 °C ISO 294
射出成形, 射出速度 200 mm/s ISO 294
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 100 °C -
Pre-drying - Time 3 h -
Processing humidity ≤0.2 % -
樹脂温度 190 - 230 °C -
金型温度 60 - 120 °C -
特殊な特性
成形加工法.
射出成形., 異形押出成形., シート押出成形., その他の押出成形.
納入形状.
ペレット.
添加剤.
離型剤.
な特性
Copolymer
領域別の利用可能性
その他の情報
村遜速揃
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min

Processing

Usual single-flighted three-section screws with an effective screw length of at least 15 D, better 20 - 23 D are suitable for the injection molding of Ultraform.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.


Postprocessing

If parts were produced at a comparatively low mold temperature (e.g. in order to obtain short cycle times) and must not change their geometry in use thermal postprocessing inducing dimensional changes by postcrystallization may be necessary. In such cases parts should be stored in an oven with recirculated air at temperatures of 100 - 130 °C until dimensions don't change significantly any further. The time needed for this has to be determined experimentally.
その他の押出成形.
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Prepreg, Melt temperature: 175 - 180 °C
Extrusion, Pipes, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
族臓遜造揃
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Profiles, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
促揃臓村促速揃
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Plates, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.