Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® Easy Slide 1 - PEEK-CF - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® Easy Slide 1:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Carbon fiber-reinforced, wear and friction modified polyether ether ketone

VESTAKEEP® Easy Slide I is a carbon fiber-reinforced, wear and friction modified polyether ether ketone for injection molding. The semi-crystalline polymer features superior, thermal and chemical resistance.
Parts made from VESTAKEEP® Easy Slide I are flame resistant and can be used for bearing bushing or gearbox parts due to the self-lubricating effect.
 
VESTAKEEP® Easy Slide I can be processed by common machines for thermoplastics.
 
We recommend a melt temperature between 380°C and 400°C during the injection molding process. The mold temperature should be within a range of 160°C to 200°C, preferably 180°C.
 
VESTAKEEP® Easy Slide I is supplied as granules in 25 kg boxes with moisture-proof polyethylene liners.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
 
For information about processing of VESTAKEEP® Easy Slide I, please follow the general recommendations in our brochure “VESTAKEEP® PEEK Processing Recommendations“.
 
Pigmentation may affect values.

The results shown have been generated from a low number of production lots. Therefore, they are preliminary and not yet the result of a statistical evaluation. Therefore they must not be used to establish specifications.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT WWW.INDUSTRIAL.VESTAKEEP.COM
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 20 cm³/10min ISO 1133
温度 380 °C -
荷重 5 kg -
成形収縮率, 平行 0.3 % ISO 294-4, 2577
成形収縮率, 直角 0.7 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 12000 MPa ISO 527
ノッチ付きシャルピー衝撃強さ, +23°C 5.5 kJ/m² ISO 179/1eA
Type of failure C - -
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 340 °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 321 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 338 °C ISO 75-1/-2
線膨張係数, 平行 10 E-6/K ISO 11359-1/-2
線膨張係数, 直角 50 E-6/K ISO 11359-1/-2
電気的特性.単位テスト基準
ISO データ
体積抵抗率 1000 Ohm*m IEC 62631-3-1
その他の特性.単位テスト基準
密度 1480 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
樹脂温度 380 - 400 °C -
金型温度 160 - 200 °C -
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット.
特殊な特性.
難燃.
な特性
Thermal Stability, Tribologic Grade
耐薬品性
General Chemical Resistance
領域別の利用可能性
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.