Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® DC 4430 G - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® DC 4430 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
X-ray opaque, white pigmented polyether ether ketone for dental applications

VESTAKEEP® DC4430 G is a white pigmented high viscosity polyether ether ketone (PEEK) resin that is especially designed for removable and fixed dentures, crowns and bridges.

VESTAKEEP® DC4430 G contains 6% Barium sulphate to render it x-ray opaque. 

Biocompatibility of VESTAKEEP® Dental
For VESTAKEEP® DC4430 G, biocompatibility has been tested according to ISO 10993-1 recommendations for permanent mucous membrane contact. The compound composition is optimised for high biocompatibility and superior mechanical, thermal and chemical resistance.
 
Biocompatibility test reports available for VESTAKEEP® DC4430 G
Standard Description
ISO 10993-03 Genotoxicity: Salmonella Typhimurium Reverse Mutation Test (Ames Test)
ISO 10993-05 Cytotoxicity: Quantitative Growth Inhibition Test
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-10 Sensitization: Local Lymph Node Assay
ISO 10993-11 Acute Systemic Toxicity
ISO 10993-11 Subacute / Subchronic Toxicity 14 days
ISO 10993-18 Extraction Tests
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation


Processing of VESTAKEEP® Dental
VESTAKEEP® DC4430 G can be processed by common melt processing techniques like injection molding and extrusion.
For injection molding, we recommend a melt temperature in the 380°C to 400°C range. The mold temperature should be within 160°C to 200°C, preferably 180°C.


Delivery of VESTAKEEP® Dental
VESTAKEEP® DC4430 G is supplied as granules in 25 kg boxes with moisture-proof polyethylene liners.

The values presented are typical or average values, they do not constitute a specification. 
 
FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY 


 
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 11 cm³/10min ISO 1133
温度 380 °C -
荷重 5 kg -
成形収縮率, 平行 1.1 % ISO 294-4, 2577
成形収縮率, 直角 1.1 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 4100 MPa ISO 527
降伏応力 95 MPa ISO 527
降伏ひずみ 4.8 % ISO 527
破壊呼びひずみ 20 % ISO 527
シャルピー衝撃強さ, +23°C N kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C N kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 6.8 kJ/m² ISO 179/1eA
Type of failure C - -
ノッチ付きシャルピー衝撃強さ, -30°C 6 kJ/m² ISO 179/1eA
Type of failure C - -
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 337 °C ISO 11357-1/-3
ガラス転移点, 10°C/min 153 °C ISO 11357-1/-2
荷重たわみ温度, 1.80 MPa 155 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 210 °C ISO 75-1/-2
ビカット軟化温度, B 305 °C ISO 306
線膨張係数, 平行 45 E-6/K ISO 11359-1/-2
その他の特性.単位テスト基準
吸水率 0.4 % Sim. to ISO 62
密度 1500 kg/m³ ISO 1183
試験片の成形条件.単位テスト基準
ISO データ
射出成形, 樹脂温度 385 °C ISO 294
射出成形, 金型温度 180 °C ISO 294
射出成形, 射出速度 200 mm/s ISO 294
特殊な特性
成形加工法.
射出成形., その他の押出成形.
納入形状.
ペレット., 白
な特性
Thermal Stability
耐薬品性
General Chemical Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved
アプリケーション
医療の
領域別の利用可能性
北アメリカ., ヨーロッパ., アジア/太平洋地域., 南・中央アメリカ., 近東/アフリカ
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com