Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® L2124 BK 9.7507 - PA12 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® L2124 BK 9.7507:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
High viscosity, plasticized, heat and light stabilized PA12 Compound

VESTAMID® L2124 BK 9.7507 is a plasticized, heat- and light- stabilized polyamide 12 compound for the extrusion of flexible tubing and hoses especially for oil and petrochemical applications. Tubing according to DIN 73 378, Type: PA 12-PHL.

Properties of compounds based on PA 12 vary little with changing humidity due to low moisture absorption. Parts made of this semi-crystalline material are characterized by exceptional impact strength, low coefficient of friction and good chemical resistance.

VESTAMID® L2124 BK 9.7507 is characterized by a high melt viscosity and good dimensional control during pipe extrusion.

VESTAMID® L2124 BK 9.7507 is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 


The values presented are typical or average values, they do not constitute a specification.


FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM
Processing/Physical Characteristics乾燥/調湿単位テスト基準
ISO データ
メルトボリュームレイト, MVR 9 / * cm³/10min ISO 1133
温度 230 / * °C -
荷重 5 / * kg -
成形収縮率, 平行 0.7 / * % ISO 294-4, 2577
成形収縮率, 直角 1.3 / * % ISO 294-4, 2577
機械的特性乾燥/調湿単位テスト基準
ISO データ
引張弾性率 400 / 420 MPa ISO 527
降伏応力 28 / 27 MPa ISO 527
降伏ひずみ 33 / 29 % ISO 527
破壊呼びひずみ >50 / >50 % ISO 527
引張クリープ弾性率, 1h * / 310 MPa ISO 899-1
引張クリープ弾性率, 1000h * / 290 MPa ISO 899-1
シャルピー衝撃強さ, +23°C N / N kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C N / N kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 150 / N kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 6 / 7 kJ/m² ISO 179/1eA
Type of failure C / C - -
熱的特性乾燥/調湿単位テスト基準
ISO データ
溶融温度, 10°C/min 171 / * °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 45 / * °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 98 / * °C ISO 75-1/-2
ビカット軟化温度, B 125 / * °C ISO 306
線膨張係数, 平行 170 / * E-6/K ISO 11359-1/-2
線膨張係数, 直角 160 / * E-6/K ISO 11359-1/-2
1.5mm厚さでの燃焼性 HB / * class IEC 60695-11-10
試験片の厚さ 1.6 / * mm -
電気的特性.乾燥/調湿単位テスト基準
ISO データ
比誘電率, 100Hz 12 / 15 - IEC 62631-2-1
比誘電率, 1MHz 3.8 / 4.1 - IEC 62631-2-1
誘電正接, 100Hz 1600 / 1600 E-4 IEC 62631-2-1
誘電正接, 1MHz 1500 / 1900 E-4 IEC 62631-2-1
体積抵抗率 1E10 / 1E9 Ohm*m IEC 62631-3-1
表面抵抗率 * / 2E13 Ohm IEC 62631-3-2
耐電圧 37 / 30 kV/mm IEC 60243-1
耐トラッキング性 600 / 600 - IEC 60112
その他の特性.乾燥/調湿単位テスト基準
吸水率 1.3 / * % Sim. to ISO 62
吸湿率 0.5 / * % Sim. to ISO 62
密度 1030 / 1030 kg/m³ ISO 1183
試験片の成形条件.単位テスト基準
ISO データ
射出成形, 樹脂温度 220 °C ISO 294
射出成形, 金型温度 60 °C ISO 294
射出成形, 射出速度 200 mm/s ISO 294
射出成形, 保圧 70 MPa ISO 294
機能
 応力-ひずみ. , VESTAMID® L2124 BK 9.7507 (乾燥), PA12, Evonik
 割線弾性率−ひずみ. , VESTAMID® L2124 BK 9.7507 (乾燥), PA12, Evonik
 応力-ひずみ (等時的). 23°C, VESTAMID® L2124 BK 9.7507 (調湿), PA12, Evonik
 クリープ弾性率−時間. 23°C, VESTAMID® L2124 BK 9.7507 (調湿), PA12, Evonik
クリープ曲線 23°C, VESTAMID® L2124 BK 9.7507 (調湿), PA12, Evonik
 引張弾性率-温度. , VESTAMID® L2124 BK 9.7507 (乾燥), PA12, Evonik
特殊な特性
成形加工法.
射出成形., Pipe/Tube Extrusion, 異形押出成形., その他の押出成形.
納入形状.
ペレット., 黒
添加剤.
滑剤., 可塑剤.
特殊な特性.
高耐衝撃及び耐衝撃改良., 光安定化., 紫外線安定化., 熱安定化.
な特性
Tribologic Grade
耐薬品性
General Chemical Resistance, Oil Resistance
領域別の利用可能性
北アメリカ., ヨーロッパ., アジア/太平洋地域., 南・中央アメリカ., 近東/アフリカ
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com