Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Eastar™ MN210 - Copolyester - Eastman Chemical Co.

Material Data Center offers the following functions for Eastar™ MN210:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Eastar datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文

Meets ISO 10993 and/or USP Class VI biocompatibility requirement.

Eastar™ Copolyester MN210, Natural is a brilliantly clear polymer with good impact strength, chemical resistance, dimensional stability, and low shrinkage rates. The slower rate of crystallization of this material makes it excellent for use in hot runner systems with valve or thermal gates.




Processing/Physical Characteristics単位テスト基準
ASTM数据
成形収縮率., 平行 0.0035 mm/mm ASTM D 955
機械的特性単位テスト基準
ASTM数据
降伏応力 50 MPa ASTM D 638
破壊応力 28 MPa ASTM D 638
降伏点伸び 4 % ASTM D 638
破断伸び 110 % ASTM D 638
曲げ弾性率 2100 MPa ASTM D 790
曲げ強さ 70 MPa ASTM D 790
ロックウェル硬度 106 - ASTM D 785
ノッチ付きIzod衝撃強さ, 1/8 in 101 J/m ASTM D 256
ノッチ付きIzod衝撃強さ, Low-Temperature 37 J/m ASTM D 256
温度 -40 °C -
アイゾット衝撃試験, 1/8 in N J/m ASTM D 256
熱的特性単位テスト基準
ASTM数据
DTUL @ 66 psi 70 °C ASTM D 648
DTUL @ 264 psi 63 °C ASTM D 648
ビカット軟化温度 85 °C ASTM D 1525
熱伝導率, ソリッド 0.0274 W/(m K) ASTM C 177
その他の特性.単位テスト基準
吸水率, 24hr 0.13 % ASTM D 570
密度 1270 kg/m³ ASTM D 792
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 70 °C -
Pre-drying - Time 6 h -
樹脂温度 250 - 270 °C -
金型温度 15 - 30 °C -
特殊な特性
成形加工法.
射出成形.
納入形状.
ナチュラルカラー
特殊な特性.
高耐衝撃及び耐衝撃改良., 滅菌可能, Gamma irradiation sterilization, Electron beam (e-beam) sterilization
な特性
Color Stability, Copolymer
耐薬品性
General Chemical Resistance, Solvent Resistance, Radiation Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved
アプリケーション
医療の
領域別の利用可能性
北アメリカ., ヨーロッパ., アジア/太平洋地域., 南・中央アメリカ., 近東/アフリカ
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.