Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of INNOPRENE 1800 N - TPE - Kumho Polychem

Material Data Center offers the following functions for INNOPRENE 1800 N:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Innoprene datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
機械的特性単位テスト基準
ISO データ
引張強度 9.81 MPa ISO 37
圧縮永久ひずみ 70℃, 24h 45 % ISO 815
引裂強さ 49 kN/m ISO 34-1
ショア硬さA 80 - ISO 7619-1
ASTM数据
伸び率100%弾性率 3.4 MPa ASTM D 412
ショア硬さA 80 - ASTM D 2240
引裂強さ 49 kN/m ASTM D 624
圧縮永久ひずみ, 22 hr @ 158 °F 45 % ASTM D 395
引張強度 9.81 MPa ASTM D 412
その他の特性.単位テスト基準
密度. 960 kg/m³ ISO 1183
密度 960 kg/m³ ASTM D 792
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 85 °C -
Pre-drying - Time 3 h -
樹脂温度 190 - 230 °C -
金型温度 10 - 60 °C -
Zone 1 160 - 180 °C -
Zone 2 180 - 200 °C -
Zone 3 200 °C -
Nozzle temperature 200 - 220 °C -
Processing Recommendation Extrusion単位テスト基準
Pre-drying - Temperature 85 °C -
Pre-drying - Time 3 h -
樹脂温度 190 - 230 °C -
Feed temperature 160 - 170 °C -
Zone 1 180 - 200 °C -
Zone 2 180 - 200 °C -
Zone 3 180 - 200 °C -
Nozzle temperature 180 - 210 °C -
特殊な特性
成形加工法.
射出成形., Pipe/Tube Extrusion, 異形押出成形., シート押出成形., Wire/Cable Extrusion, ブロー成形., カレンダー加工.
納入形状.
ペレット., ナチュラルカラー
特殊な特性.
紫外線安定化., 熱安定化.
な特性
Fatigue Resistance
耐薬品性
General Chemical Resistance, Ozone Resistance
アプリケーション
汎用
領域別の利用可能性
アジア/太平洋地域.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.