Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Novodur® HD-15 - ABS - INEOS Styrolution

Material Data Center offers the following functions for Novodur® HD-15:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, CAE Interfaces

Check here, which other Novodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Novodur® HD 15 acrylonitrile butadiene styrene (ABS) polymer features high surface quality and good impact strength. Novodur® HD 15 is an easily processable ABS grade with well-balanced mechanical properties and an excellent chemical and stress cracking resistance. Medical and food contact statements are available upon request.
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 15 cm³/10min ISO 1133
温度 220 °C -
荷重 10 kg -
溶融時の密度 940 kg/m³ -
溶融時の熱伝導率 0.241 W/(m K) -
溶融時の比熱 2230 J/(kg K) -
突き出し時の時の温度 90 °C -
機械的特性単位テスト基準
ISO データ
引張弾性率 2300 MPa ISO 527
降伏応力 48 MPa ISO 527
降伏ひずみ 2.5 % ISO 527
破壊呼びひずみ 10 % ISO 527
シャルピー衝撃強さ, +23°C 170 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 90 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 14 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 6 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
荷重たわみ温度, 1.80 MPa 93 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 99 °C ISO 75-1/-2
ビカット軟化温度, B 100 °C ISO 306
線膨張係数, 平行 90 E-6/K ISO 11359-1/-2
電気的特性.単位テスト基準
ISO データ
耐電圧 37 kV/mm IEC 60243-1
耐トラッキング性 600 - IEC 60112
その他の特性.単位テスト基準
吸水率 1 % Sim. to ISO 62
吸湿率 0.22 % Sim. to ISO 62
密度 1050 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 80 °C -
Pre-drying - Time 2 - 4 h -
樹脂温度 220 - 260 °C -
金型温度 30 - 60 °C -
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット.
特殊な特性.
滅菌可能, エチレンオキシド滅菌(EtO), Gamma irradiation sterilization
耐薬品性
Radiation Resistance
Certifications
Food contact, Food approval 10/2011, Food approval FDA 21 CFR, Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved, Drug Master File, Long term supply assurance
アプリケーション
医療の
領域別の利用可能性
ヨーロッパ., アジア/太平洋地域., 近東/アフリカ
その他の情報
村遜速揃
PREPROCESSING

Pre-drying, Temperature: 80°C

Pre-drying, Time: 2 - 4h

PROCESSING

Melt temperature, range: 230 - 260°C

Mold temperature, range: 60 - 80°C

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.