Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of RTP 800 TFE 2 UV - (POM+PTFE) - RTP Company

Material Data Center offers the following functions for RTP 800 TFE 2 UV:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other RTP datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristics単位テスト基準
ASTM数据
成形収縮率., 平行 0.0265 mm/mm ASTM D 955
機械的特性単位テスト基準
ASTM数据
引張弾性率 2551 MPa ASTM D 638
引張強度 55.2 MPa ASTM D 638
曲げ弾性率 2344 MPa ASTM D 790
曲げ強さ 79.3 MPa ASTM D 790
ノッチ付きIzod衝撃強さ, 1/8 in 80.1 J/m ASTM D 256
熱的特性単位テスト基準
ASTM数据
UL94 燃焼性 HB - UL 94
追加試験片の厚さ 1.59 mm -
DTUL @ 264 psi 107 °C ASTM D 648
電気的特性.単位テスト基準
ASTM数据
体積抵抗率 >1E15 Ohm*cm ASTM D 257
その他の特性.単位テスト基準
密度 1420 kg/m³ ASTM D 792
Moisture Content 0.15 % -
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 121 °C -
Pre-drying - Time 2 h -
樹脂温度 182 - 218 °C -
金型温度 79.4 - 107 °C -
Injection pressure 68.9 - 103 MPa -
特殊な特性
成形加工法.
射出成形.
添加剤.
滑剤.
特殊な特性.
紫外線安定化.
領域別の利用可能性
北アメリカ., ヨーロッパ., アジア/太平洋地域.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com