Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Rilsamid® AZM 23 BLACK T6LD - PA12-GF23 - ARKEMA

Material Data Center offers the following functions for Rilsamid® AZM 23 BLACK T6LD:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Rilsamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
ISO 16396 - PA12, GF23, M1GHLR, 16-060

Rilsamid® AZM 23 BLACK T6LD resin is a fiberglass reinforced polyamide. 
This black colored grade is designed for injection moulding.


Packaging: 
This grade is delivered dried in sealed packaging (25 kg bags / 450 kg rigid containers) ready to be processed

Shelf life: 
Two years from the delivery.
For any use above this limit please refer to our technical services. 
Processing/Physical Characteristics乾燥/調湿単位テスト基準
ISO データ
メルトボリュームレイト, MVR 13 / * cm³/10min ISO 1133
温度 235 / * °C -
荷重 5 / * kg -
成形収縮率, 平行 0.2 / * % ISO 294-4, 2577
成形収縮率, 直角 0.4 / * % ISO 294-4, 2577
機械的特性乾燥/調湿単位テスト基準
ISO データ
引張弾性率 5500 / 5070 MPa ISO 527
破壊応力 95 / 100 MPa ISO 527
破壊ひずみ 5 / 5.2 % ISO 527
シャルピー衝撃強さ, +23°C 66 / 77 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 66 / 83 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 15 / 19 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 8 / 12 kJ/m² ISO 179/1eA
熱的特性乾燥/調湿単位テスト基準
ISO データ
溶融温度, 10°C/min 179 / * °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 165 / * °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 173 / * °C ISO 75-1/-2
ビカット軟化温度, B 165 / * °C ISO 306
線膨張係数, 平行 60 / * E-6/K ISO 11359-1/-2
電気的特性.乾燥/調湿単位テスト基準
ISO データ
比誘電率, 100Hz 5 / - - IEC 62631-2-1
比誘電率, 1MHz 5 / - - IEC 62631-2-1
誘電正接, 100Hz 1170 / - E-4 IEC 62631-2-1
誘電正接, 1MHz 364 / - E-4 IEC 62631-2-1
その他の特性.乾燥/調湿単位テスト基準
吸水率 1.3 / * % Sim. to ISO 62
吸湿率 0.5 / * % Sim. to ISO 62
密度 1180 / 1170 kg/m³ ISO 1183
機能
 粘度せん断速度. , Rilsamid® AZM 23 BLACK T6LD, PA12-GF23, ARKEMA
 せん断応力-せん断速度. , Rilsamid® AZM 23 BLACK T6LD, PA12-GF23, ARKEMA
 せん断弾性率-温度. , Rilsamid® AZM 23 BLACK T6LD (乾燥), PA12-GF23, ARKEMA
 応力-ひずみ. , Rilsamid® AZM 23 BLACK T6LD (乾燥), PA12-GF23, ARKEMA
 割線弾性率−ひずみ. , Rilsamid® AZM 23 BLACK T6LD (乾燥), PA12-GF23, ARKEMA
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット., 黒
添加剤.
離型剤.
特殊な特性.
光安定化., 紫外線安定化., 熱安定化.
領域別の利用可能性
その他の情報
村遜速揃

Processing conditions:

- Typical melt temperature (Min / Recommended / Max) : 250°C / 265°C / 280°C.
- Typical mold temperature : 40 – 90°C.
- Drying time and temperature (only necessary for bags opened for more than two hours) : 4-8 hours at 80-90°C.

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.