Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultradur® B 4335 G3 HR High Speed - PBT-I-GF15 - BASF

Material Data Center offers the following functions for Ultradur® B 4335 G3 HR High Speed:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultradur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Easy flowing, impact modified injection-molding grade containing 15% glass-fibers, for technical parts with highest demands on hydrolysis resistance such as sensors or connectors in engine compartments.
The black colored product Ultradur® B4335 G3 HR High Speed BK15126 has a LS coloration (Laser Sensitive) and can be marked with Nd:YAG lasers.

Abbreviated designation according to ISO 1043-1: PBT-I-GF15
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 25 cm³/10min ISO 1133
温度 275 °C -
荷重 2.16 kg -
成形収縮率, 平行 0.7 % ISO 294-4, 2577
成形収縮率, 直角 1.0 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
引張弾性率 4700 MPa ISO 527
破壊応力 90 MPa ISO 527
破壊ひずみ 3.5 % ISO 527
曲げ弾性率, 23°C 4300 MPa ISO 178
曲げ強さ 135 MPa ISO 178
シャルピー衝撃強さ, +23°C 55 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 32 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 11 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 7 kJ/m² ISO 179/1eA
熱的特性単位テスト基準
ISO データ
溶融温度, 10°C/min 223 °C ISO 11357-1/-3
荷重たわみ温度, 1.80 MPa 200 °C ISO 75-1/-2
荷重たわみ温度, 0.45 MPa 220 °C ISO 75-1/-2
線膨張係数, 平行 40 E-6/K ISO 11359-1/-2
厚さhでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 0.8 mm -
電気的特性.単位テスト基準
ISO データ
体積抵抗率 1E13 Ohm*m IEC 62631-3-1
表面抵抗率 1E15 Ohm IEC 62631-3-2
耐電圧 38 kV/mm IEC 60243-1
耐トラッキング性 600 - IEC 60112
その他の特性.単位テスト基準
密度 1360 kg/m³ ISO 1183
Bulk density 750 kg/m³ -
材料特有の特性単位テスト基準
ISO データ
粘度数 90 cm³/g ISO 307, 1157, 1628
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 80 - 120 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.04 % -
樹脂温度 250 - 280 °C -
金型温度 60 - 100 °C -
Processing Recommendation Extrusion単位テスト基準
Processing humidity ≤0.04 % -
樹脂温度 250 - 280 °C -
機能
 応力-ひずみ. , Ultradur® B 4335 G3 HR High Speed, PBT-I-GF15, BASF
 割線弾性率−ひずみ. , Ultradur® B 4335 G3 HR High Speed, PBT-I-GF15, BASF
 引張弾性率-温度. , Ultradur® B 4335 G3 HR High Speed, PBT-I-GF15, BASF
特殊な特性
成形加工法.
射出成形., その他の押出成形.
納入形状.
ナチュラルカラー
特殊な特性.
高耐衝撃及び耐衝撃改良.
耐薬品性
Hydrolytically Stable
アプリケーション
自動車
領域別の利用可能性
北アメリカ., ヨーロッパ.
その他の情報
村遜速揃
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 280 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 60 - 100 °C
injection molding, Mold temperature, recommended: 80 °C
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.