Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of IMPET® 340R - PET-GF45 - Celanese

Material Data Center offers the following functions for IMPET® 340R:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Impet datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Impet 340R is a 45% glass-reinforced injection moldable polyester made with post consumer recycled PET. It provides an excellent combination of strength, stiffness, and high temperature resistance.

Flammability at thickness h (0.81 mm)HB-
Processing/Physical Characteristics단위시험규격
ISO 데이터
성형 수축률, 평행 0.2 % ISO 294-4, 2577
성형 수축률, 수직 0.6 % ISO 294-4, 2577
기계적 특성단위시험규격
ISO 데이터
인장탄성률 16800 MPa ISO 527
파단시 강도 175 MPa ISO 527
파단시 신율 1.7 % ISO 527
챠피 충격 강도 , +23°C 24 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 21 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 11 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 9 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 244 °C ISO 11357-1/-3
유리 전이 온도, 10 °C/min 73 °C ISO 11357-1/-2
하중하에서의 변형온도, 1.80 MPa 229 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 240 °C ISO 75-1/-2
선형 열팽창 계수, 평행 14 E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 83 E-6/K ISO 11359-1/-2
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 0.8 mm -
산소지수로서의 난연성 22 % ISO 4589-1/-2
전기적 특성단위시험규격
ISO 데이터
부피 저항 >1E13 Ohm*m IEC 62631-3-1
기타 특성단위시험규격
밀도 1730 kg/m³ ISO 1183
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 121 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.01 % -
용융수지온도 270 - 300 °C -
성형온도 110 - 120 °C -
특징
생산 공정
사출 성형
인도 유형
펠렛 (입자,알갱이)
부가물
윤활제
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧, 쨀짼쨘횓 쨔횞 횁횩쩐횙 쩐횈쨍횧쨍짰횆짬, 쨉쩔쩐챌 쨔횞 쩐횈횉횁쨍짰횆짬 짹횢쩔짧
기타 정보
사E성
To avoid hydrolytic degradation during processing, IMPET resins have to be dried to a moisture level equal to or less than 0.01%. Drying should be done in a dehumidifying hopper dryer capable of dewpoints <-30°F (-34°C) at 275°F (121°C) for 4 hours.
Rear Temperature 500-520(260-270) deg F (deg C)
Center Temperature 520-530(270-275) deg F (deg C)
Front Temperature 530-540(275-280) deg F (deg C)
Nozzle Temperature 530-550(275-290) deg F (deg C)
Melt Temperature 520-570(270-300) deg F (deg C)
Mold Temperature 230-250(110-120) deg F (deg C)
Back Pressure 0-25 psi
Screw Speed 50-75 rpm
Injection Speed Medium/Fast

Injection speed, injection pressure and holding pressure have to be optimized to the individual article geometry. To avoid material degradation during processing low back pressure and minimum screw speed have to be used. Overheating of the material has to be avoided, in particular for flame retardant grades. Up to 25% clean and dry regrind may be used.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.