Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox. Information about Biopolymers, a project by FH Hannover and M-Base Engineering & Software GmbH sponsored by Fachagentur Nachwachsende Rohstoffe (FNR).

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Novodur® ECO P2H-AT BC50 - ABS - INEOS Styrolution

Material Data Center offers the following functions for Novodur® ECO P2H-AT BC50:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Novodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Novodur® ECO P2H-AT BC50 as acrylonitrile butadiene styrene (ABS) polymer features high surface quality and good impact strength. Novodur® ECO P2H-AT BC50 is a general purpose injection molding grade with enhanced chemical resistance and contains an antistatic additive. It is designed for best aesthetics: stable high gloss and smooth finish. Novodur® ECO P2H-AT BC50 is an ISCC compliant product leading to a substitution of fossil source styrene with ISCC certified bio-attributed styrene.
Carbon Footprint Reduction vs Fossil-Based (3rd party validated): 68 % (ISO 14044)
Attributed Content of ISCC-certified Bio-Circular Sources (min.): 50 %
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 37 cm³/10min ISO 1133
온도 220 °C -
하중 10 kg -
성형 수축률, 평행 0.6 % ISO 294-4, 2577
용융 열전도율 0.129 W/(m K) -
용융 비열용량 1800 J/(kg K) -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 2500 MPa ISO 527
항복강도 44 MPa ISO 527
항복변형률 2.1 % ISO 527
파단시 평균신율 18 % ISO 527
굴곡 계수, 23°C 2400 MPa ISO 178
굴곡 강도 70 MPa ISO 178
챠피 충격 강도 , +23°C 100 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 80 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 18 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 8 kJ/m² ISO 179/1eA
아이조드 충격은 노치, +23°C 18 kJ/m² ISO 180/1A
아이조드 충격은 노치 9 kJ/m² ISO 180/1A
온도 -30 °C -
Ball indentation hardness 110 MPa ISO 2039-1
열적 특성단위시험규격
ISO 데이터
하중하에서의 변형온도, 1.80 MPa 93 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 97 °C ISO 75-1/-2
비카트 연화 온도, B 98 °C ISO 306
선형 열팽창 계수, 평행 90 E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 HB class IEC 60695-11-10
테스트 두께 1.5 mm -
Yellow Card 유효한 - -
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 3.0 mm -
Yellow Card 유효한 - -
연소속도, FMVSS, 두께 1mm 60[1] mm/min ISO 3795 (FMVSS 302)
Glow Wire Flammability Index (GWFI) 700 °C IEC 60695-2-12
GWFI - thickness tested (1) 2 mm -
1: 2 mm
전기적 특성단위시험규격
ISO 데이터
전기 압력 34 kV/mm IEC 60243-1
CTI 600 - IEC 60112
기타 특성단위시험규격
밀도 1050 kg/m³ ISO 1183
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 80 °C -
Pre-drying - Time 2 - 4 h -
용융수지온도 230 - 260 °C -
성형온도 60 - 80 °C -
도표
점도-변형률 , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
전단-변형률 , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
동전단탄성율-온도 , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
응력-신율 , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
시컨트탄성율-신율 , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
응력-신율(등시) 23°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
크립탄성율-시간 23°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
곡선 크리프 23°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
응력-신율(등시) 40°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
크립탄성율-시간 40°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
곡선 크리프 40°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
응력-신율(등시) 60°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
크립탄성율 -시간 60°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
곡선 크리프 60°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
응력-신율(등시) 80°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
크립탄성율-시간 80°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
곡선 크리프 80°C, Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
비용적-온도(pvT) , Novodur® ECO P2H-AT BC50, ABS, INEOS Styrolution
특징
생산 공정
사출 성형
인도 유형
펠렛 (입자,알갱이)
특별 특성
정전기 방지, 고충격 또는 고충격 보강
특성
High Gloss
내화학성에
General Chemical Resistance
Certifications
Contains renewable resources, ISCC Plus
응용
전기 및 전자 , 범용, 포장
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧, 쨀짼쨘횓 쨔횞 횁횩쩐횙 쩐횈쨍횧쨍짰횆짬, 쨉쩔쩐챌 쨔횞 쩐횈횉횁쨍짰횆짬 짹횢쩔짧
기타 정보
사E성
PREPROCESSING

Pre-drying, Temperature: 80°C

Pre-drying, Time: 2 - 4h

PROCESSING

Melt temperature, range: 230 - 260°C

Mold temperature, range: 60 - 80°C

Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.