Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of POLYFORT® FPP 30 GFC K1079 - PP-GF30 - LyondellBasell Industries

Material Data Center offers the following functions for POLYFORT® FPP 30 GFC K1079:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Polyfort datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서

30% chemical coupled glass fibre reinforced PP-homopolymer; long term heat stabilized; meets VW-TL PP10


Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 5 cm³/10min ISO 1133
온도 230 °C -
하중 2.16 kg -
성형 수축률, 평행 0.2 % ISO 294-4, 2577
성형 수축률, 수직 1.2 % ISO 294-4, 2577
용융 밀도 970 kg/m³ -
용융 열전도율 0.155 W/(m K) -
용융 비열용량 2000 J/(kg K) -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 6700 MPa ISO 527
파단시 강도 85 MPa ISO 527
파단시 신율 3 % ISO 527
챠피 충격 강도 , +23°C 48 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 45 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 9 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 8 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 168 °C ISO 11357-1/-3
하중하에서의 변형온도, 1.80 MPa 145 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 159 °C ISO 75-1/-2
비카트 연화 온도, B 131 °C ISO 306
선형 열팽창 계수, 평행 25 E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 95 E-6/K ISO 11359-1/-2
선형 온도 팽창 계수 (-40도에서 100도), 평행 20 E-6/K ISO 11359-1/-2
선형 온도 팽창 계수 (-40도에서 100도), 평행 115 E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 HB class IEC 60695-11-10
테스트 두께 1.5 mm -
Yellow Card 유효한 - -
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 3.0 mm -
Yellow Card 유효한 - -
연소속도, FMVSS, 두께 1mm 50 mm/min ISO 3795 (FMVSS 302)
전기적 특성단위시험규격
ISO 데이터
부피 저항 >1E13 Ohm*m IEC 62631-3-1
표면 저항 >1E15 Ohm IEC 62631-3-2
기타 특성단위시험규격
밀도 1130 kg/m³ ISO 1183
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 80 °C -
Pre-drying - Time 2 - 4 h -
용융수지온도 230 - 270 °C -
성형온도 40 - 70 °C -
도표
점도-변형률 , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
전단-변형률 , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
응력-신율 , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
시컨트탄성율-신율 , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
비용적-온도(pvT) , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
인장탄성율-온도 , POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
LTHA-파단시 신율  4mm, POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
LTHA-챠피 충격 강도 (23°C) 4mm, POLYFORT® FPP 30 GFC K1079, PP-GF30, LyondellBasell
특징
생산 공정
사출 성형
인도 유형
과립
부가물
이형제
특별 특성
U.V. 안정성 또는 기후 안정성, 열안정성
지역별 검색
기타 정보
사E성
PREPROCESSING; Pretreatment
Predrying usually not neccessary (2-4h / 80°C)

PROCESSING ;Processing:

Melttemperature230 - 270°C
Mouldtemperature40 - 70°C
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.