Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultradur® B 4300 GM42 - PBT-(GF+MF)30 - BASF

Material Data Center offers the following functions for Ultradur® B 4300 GM42:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultradur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Injection molding grade, containing a glass fiber and mineral reinforcement, for parts with good surface finish and stiffness, as well as low warpage tendency (e.g.housings).

Abbreviated designation according to ISO 1043: PBT-GF20 M10
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 17 cm³/10min ISO 1133
온도 250 °C -
하중 2.16 kg -
성형 수축률, 평행 0.5 % ISO 294-4, 2577
성형 수축률, 수직 1.2 % ISO 294-4, 2577
기계적 특성단위시험규격
ISO 데이터
인장탄성률 7900 MPa ISO 527
파단시 강도 105 MPa ISO 527
파단시 신율 2.7 % ISO 527
탄성변형률, 1000h 4500 MPa ISO 899-1
챠피 충격 강도 , +23°C 45 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 43 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 4.5 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 223 °C ISO 11357-1/-3
하중하에서의 변형온도, 1.80 MPa 195 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 220 °C ISO 75-1/-2
1.5mm 평균두께에서의 난연성 HB class IEC 60695-11-10
테스트 두께 1.5 mm -
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 0.8 mm -
산소지수로서의 난연성 21 % ISO 4589-1/-2
전기적 특성단위시험규격
ISO 데이터
상대 유전율, 100Hz 3.8 - IEC 62631-2-1
상대 유전뮬, 1MHz 3.8 - IEC 62631-2-1
소산 인자, 100Hz 12 E-4 IEC 62631-2-1
소산 인자, 1MHz 150 E-4 IEC 62631-2-1
부피 저항 >1E13 Ohm*m IEC 62631-3-1
표면 저항 1E13 Ohm IEC 62631-3-2
CTI 300 - IEC 60112
기타 특성단위시험규격
물에서의 흡수성 0.4 % ISO 62와 유사
조건에서의 흡습성 0.2 % ISO 62와 유사
밀도 1550 kg/m³ ISO 1183
물질의 비성질단위시험규격
ISO 데이터
점도수 101 cm³/g ISO 307, 1157, 1628
테스트 견본 생산단위시험규격
ISO 데이터
사출성형: 용융수지온도 250 °C ISO 294
사출성형: 금형온도 80 °C ISO 294
사출성형: 사출속도 200 mm/s ISO 294
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 80 - 120 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.04 % -
용융수지온도 250 - 275 °C -
성형온도 60 - 90 °C -
도표
점도-변형률 , Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
전단-변형률 , Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율 , Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
시컨트탄성율-신율 , Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 23°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율-시간 23°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 23°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 40°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율-시간 40°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 40°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 60°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율 -시간 60°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 60°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 90°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율-시간 90°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 90°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 120°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율-시간 120°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 120°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
응력-신율(등시) 160°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
크립탄성율- 시간 160°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
곡선 크리프 160°C, Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
인장탄성율-온도 , Ultradur® B 4300 GM42, PBT-(GF+MF)30, BASF
특징
생산 공정
사출 성형
인도 유형
펠렛 (입자,알갱이)
부가물
윤활제
특별 특성
가시광선 안정성, U.V. 안정성 또는 기후 안정성, 열안정성
지역별 검색
기타 정보
사E성
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 250 °C
injection molding, Mold temperature, range: 60 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
화학적 매체에 대한 저항력
에서의 아세트산 (질량 5%) (23°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.