Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultrason® P 3010 NAT - PPSU - BASF

Material Data Center offers the following functions for Ultrason® P 3010 NAT:
unit conversion, PDF datasheet print, comparison with other plastics, parameters for material models, CAE Interfaces

Check here, which other Ultrason P datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Medium viscosity, unreinforced injection-molding and extrusion grade with superior toughness and chemical resistance (stress crack resistance), resistance against superheated steam.
Abbreviated designation according to ISO 1043-1: PPSU
Processing/Physical Characteristics건조/응축단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 35 / * cm³/10min ISO 1133
온도 360 / * °C -
하중 10 / * kg -
성형 수축률, 평행 0.9 / * % ISO 294-4, 2577
성형 수축률, 수직 1.0 / * % ISO 294-4, 2577
기계적 특성건조/응축단위시험규격
ISO 데이터
인장탄성률 - / 2250 MPa ISO 527
항복강도 - / 74 MPa ISO 527
항복변형률 - / 7.8 % ISO 527
챠피 충격 강도 , +23°C - / N kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C - / N kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C - / 70 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C - / 45 kJ/m² ISO 179/1eA
열적 특성건조/응축단위시험규격
ISO 데이터
유리 전이 온도, 10 °C/min 220 / * °C ISO 11357-1/-2
하중하에서의 변형온도, 1.80 MPa 198 / * °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 212 / * °C ISO 75-1/-2
선형 열팽창 계수, 평행 55 / * E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 V-0 / * class IEC 60695-11-10
테스트 두께 1.5 / * mm -
Yellow Card 유효한 예 / * - -
두께 H인 제품의 난연성 V-0 / * class IEC 60695-11-10
테스트 두께 3.0 / * mm -
Yellow Card 유효한 예 / * - -
산소지수로서의 난연성 43.4 / * % ISO 4589-1/-2
전기적 특성건조/응축단위시험규격
ISO 데이터
상대 유전율, 100Hz - / 3.8 - IEC 62631-2-1
상대 유전뮬, 1MHz - / 3.7 - IEC 62631-2-1
소산 인자, 100Hz - / 17 E-4 IEC 62631-2-1
소산 인자, 1MHz - / 89 E-4 IEC 62631-2-1
부피 저항 - / >1E13 Ohm*m IEC 62631-3-1
표면 저항 * / >1E15 Ohm IEC 62631-3-2
전기 압력 - / 44 kV/mm IEC 60243-1
CTI - / 150 - IEC 60112
기타 특성건조/응축단위시험규격
물에서의 흡수성 1.2 / * % ISO 62와 유사
조건에서의 흡습성 0.6 / * % ISO 62와 유사
밀도 1290 / - kg/m³ ISO 1183
물질의 비성질건조/응축단위시험규격
ISO 데이터
점도수 71 / * cm³/g ISO 307, 1157, 1628
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 140 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.02 % -
용융수지온도 350 - 390 °C -
성형온도 140 - 180 °C -
도표
응력-신율 , Ultrason® P 3010 NAT (응축), PPSU, BASF
시컨트탄성율-신율 , Ultrason® P 3010 NAT (응축), PPSU, BASF
응력-신율(등시) 23°C, Ultrason® P 3010 NAT (응축), PPSU, BASF
크립탄성율-시간 23°C, Ultrason® P 3010 NAT (응축), PPSU, BASF
곡선 크리프 23°C, Ultrason® P 3010 NAT (응축), PPSU, BASF
응력-신율(등시) 180°C, Ultrason® P 3010 NAT (건조), PPSU, BASF
크립탄성율-시간 180°C, Ultrason® P 3010 NAT (건조), PPSU, BASF
곡선 크리프 180°C, Ultrason® P 3010 NAT (건조), PPSU, BASF
비용적-온도(pvT) , Ultrason® P 3010 NAT, PPSU, BASF
인장탄성율-온도 , Ultrason® P 3010 NAT (응축), PPSU, BASF
특징
생산 공정
사출 성형, 필름 압출, 외형 압출, 시트 압출, 기타 압출, 중공 성형, 열성형
인도 유형
펠렛 (입자,알갱이), 자연 색상
특별 특성
난연성, 투명도, 멸균
특성
Melt Strength
내화학성에
General Chemical Resistance
Certifications
Food contact
응용
의료
지역별 검색
기타 정보
사E성
PREPROCESSING
Pre/Post-processing, max. allowed water content: .02 %
Pre/Post-processing, Pre-drying, Temperature: 140 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 350 - 390 °C
injection molding, Melt temperature, recommended: 370 °C
injection molding, Mold temperature, range: 140 - 180 °C
injection molding, Mold temperature, recommended: 160 °C
injection molding, Dwell time, thermoplastics: 10 min

Pretreatment
Drying temperature: 130 - 150°C
Drying time: minimum 4h
recommended dryer: vaccum or dry air dryer
maximum moisture: 0,02 - 0,05%

Ultrason® can be injection molded by any type of machinery on the market, provided that the plasticizing unit and the mold temperature control system have been configured appropriately. The machinery manufacturer must be consulted if any doubts exist on the ability of various parts to withstand the high temperatures required (e.g. barrel, barrel head, bolted connections, etc.)

Long residence time in combination with high temperatures should be avoided e.g. by pump out material at regular intervals.
During extended interruptions, the barrel temperature should be lowered to about 250-280°C.

It has been found out that heating to the requested processing temperature and shutting down or lowering the temperature is best carried out in two steps.
First, the barrel temperatures are set at the lower processing temperature range for the particular thermoplastic (340 - 350 °C). As soon as these temperatures have reached a steady state, the material in the barrel is pumped out. Second, the barrel temperature can be set to the required processing temperature or the heaters can be shut down.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.