Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® Care M40 R - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® Care M40 R:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
High viscosity, unreinforced polyether ether ketone designed for the medical device industry
VESTAKEEP® Care is the ideal materials for the fabrication of medical devices with short time contact to human blood, tissue or bone for up to 30 days. VESTAKEEP® Care Grades have a good biocompatibility, processability and the option to pigment.

VESTAKEEP® Care M40 R are semi finished goods based on the high viscosity VESTAKEEP® Care M40 G polymer resin. 

The semi-crystalline polymer features superior thermal and chemical resistance.

Biocompatibility of VESTAKEEP® Care
In an extensive testing program run by independent certified labs, biocompatibility has been tested following United States Pharmacopeia and ISO 10933-1:2003 guidelines.
The test reports attest VESTAKEEP® Care’s excellent biocompatibility.

Biocompatibility tests for VESTAKEEP® Care:

 
Delivery of VESTAKEEP® Care
VESTAKEEP® Care M40 R rods can be produced in various diameters ranging from 6 mm up to 100 mm. The standard length is 1 m. Other dimensions are also available upon request.

Mechanical properties are evaluated on stock shapes test bars and further values are evaluated on injection molded samples.
The results shown have been generated from a low number of production lots. Therefore, they are preliminary and not yet the result of a statistical evaluation. Therefore they must not be used to establish specifications.


FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 11 cm³/10min ISO 1133
온도 380 °C -
하중 5 kg -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 4050 MPa ISO 527
항복강도 110 MPa ISO 527
항복변형률 5 % ISO 527
파단시 평균신율 40 % ISO 527
쇼어 D 경도 84 - ISO 7619-1
열적 특성단위시험규격
ISO 데이터
하중하에서의 변형온도, 1.80 MPa 155 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 205 °C ISO 75-1/-2
비카트 연화 온도, B 305 °C ISO 306
선형 열팽창 계수, 평행 60 E-6/K ISO 11359-1/-2
전기적 특성단위시험규격
ISO 데이터
상대 유전뮬, 1MHz 2.8 - IEC 62631-2-1
기타 특성단위시험규격
물에서의 흡수성 0.5 % ISO 62와 유사
밀도 1300 kg/m³ ISO 1183
특징
인도 유형
Semifinished product
특성
Thermal Stability
내화학성에
General Chemical Resistance
Certifications
Medical Grade, Biocompatibility ISO 10993, US Pharmacopeia Class VI Approved
응용
의료
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧, 쨀짼쨘횓 쨔횞 횁횩쩐횙 쩐횈쨍횧쨍짰횆짬, 쨉쩔쩐챌 쨔횞 쩐횈횉횁쨍짰횆짬 짹횢쩔짧
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.