Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTODUR® X9400 - PBT-GF10 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTODUR® X9400:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Glass fiber-reinforced, modified polybutylene terephthalate compound with decreased shrinkage

VESTODUR® X9400 NC is a 10% glass fiber-reinforced, polymer-modified polybutylene terephthalate compound. Moldings of this compound show decreased shrinkage.

 

The compound is suitable for parts that are subjected to high mechanical or thermal loads. Compared with commonly used glass fiber-reinforced PBT compounds with similar stiffness parts of VESTODUR® X9400 have in particular a high surface quality.

 

VESTODUR® X9400 is supplied as cylindrical pellets in polyethylene packaging. 

For information, please follow the general recommendations in our flyer "VESTODUR® Polybutylene terephthalate - Compounds".

 

Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at tempIeratures not exceeding 30°C.
 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM 
OR VISIT OUR PRODUCT AT  WWW.VESTODUR.COM

Processing/Physical Characteristics단위시험규격
ISO 데이터
성형 수축률, 평행 0.3 % ISO 294-4, 2577
성형 수축률, 수직 0.4 % ISO 294-4, 2577
기계적 특성단위시험규격
ISO 데이터
인장탄성률 4500 MPa ISO 527
항복강도 103 MPa ISO 527
항복변형률 4 % ISO 527
파단시 평균신율 4 % ISO 527
챠피 충격 강도 , +23°C 50 kJ/m² ISO 179/1eU
Type of failure C - -
챠피 충격 강도, -30°C 45 kJ/m² ISO 179/1eU
Type of failure C - -
챠피 노치드 충격 강도, +23°C 5 kJ/m² ISO 179/1eA
Type of failure C - -
챠피 노치드 충격 강도, -30°C 5 kJ/m² ISO 179/1eA
Type of failure C - -
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 218 °C ISO 11357-1/-3
유리 전이 온도, 10 °C/min 66 °C ISO 11357-1/-2
하중하에서의 변형온도, 1.80 MPa 110 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 200 °C ISO 75-1/-2
비카트 연화 온도, B 179 °C ISO 306
선형 열팽창 계수, 평행 30 E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 40 E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 HB class IEC 60695-11-10
테스트 두께 1.6 mm -
기타 특성단위시험규격
밀도 1350 kg/m³ ISO 1183
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.