Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Vydyne® R535J NT0665 - PA66-GF35 - Ascend

Material Data Center offers the following functions for Vydyne® R535J NT0665:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vydyne datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Vydyne R535J NT0665 is a natural, 35% glass-filled, high-flow PA66 resin that is heat-stabilized with an electrically neutral heat stabilizer. It is specially designed for electrical applications requiring high dielectric strength, low conductivity and corrosion resistance.
Processing/Physical Characteristics건조/응축단위시험규격
ISO 데이터
성형 수축률, 평행 0.4 / * % ISO 294-4, 2577
성형 수축률, 수직 0.9 / * % ISO 294-4, 2577
기계적 특성건조/응축단위시험규격
ISO 데이터
인장탄성률 11600 / - MPa ISO 527
파단시 강도 209 / - MPa ISO 527
파단시 신율 2.8 / - % ISO 527
굴곡 계수, 23°C 10500 / - MPa ISO 178
굴곡 강도 300 / - MPa ISO 178
챠피 충격 강도 , +23°C 79 / - kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 68 / - kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 12 / - kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 11 / - kJ/m² ISO 179/1eA
아이조드 충격은 노치, +23°C 12 / - kJ/m² ISO 180/1A
아이조드 충격은 노치 11 / - kJ/m² ISO 180/1A
온도 -30 °C -
열적 특성건조/응축단위시험규격
ISO 데이터
녹는점, 10°C/min 260 / * °C ISO 11357-1/-3
하중하에서의 변형온도, 1.80 MPa 251 / * °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 261 / * °C ISO 75-1/-2
선형 열팽창 계수, 평행 21 / * E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 106 / * E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 HB / * class IEC 60695-11-10
테스트 두께 1.5 / * mm -
두께 H인 제품의 난연성 HB / * class IEC 60695-11-10
테스트 두께 0.8 / * mm -
Glow Wire Flammability Index (GWFI) 750 °C IEC 60695-2-12
GWFI - thickness tested (1) 0.75 mm -
Glow Wire Flammability Index (GWFI) 725 °C IEC 60695-2-12
GWFI - thickness tested (2) 1.5 mm -
Glow Wire Flammability Index (GWFI) 800 °C IEC 60695-2-12
GWFI - thickness tested (3) 3 mm -
Glow Wire Ignition Temperature (GWIT) 775 °C IEC 60695-2-13
GWIT - thickness tested (1) 0.75 mm -
Glow Wire Ignition Temperature (GWIT) 725 °C IEC 60695-2-13
GWIT - thickness tested (2) 1.5 mm -
Glow Wire Ignition Temperature (GWIT) 750 °C IEC 60695-2-13
GWIT - thickness tested (3) 3 mm -
ASTM 데이터
UL94 난연성 HB - UL 94
테스트 두께 0.75 mm -
전기적 특성건조/응축단위시험규격
ISO 데이터
부피 저항 1E12 / - Ohm*m IEC 62631-3-1
전기 압력 20 / - kV/mm IEC 60243-1
CTI 600 / - - IEC 60112
ASTM 데이터
아크 저항 150 / - s ASTM D 495
기타 특성건조/응축단위시험규격
물에서의 흡수성 0.8 / * % ISO 62와 유사
조건에서의 흡습성 1.6 / * % ISO 62와 유사
밀도 1410 / - kg/m³ ISO 1183
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
용융수지온도 285 - 305 °C -
성형온도 65 - 95 °C -
Zone 1 280 - 310 °C -
Zone 2 280 - 310 °C -
Zone 3 280 - 310 °C -
Nozzle temperature 280 - 310 °C -
특징
생산 공정
사출 성형
인도 유형
펠렛 (입자,알갱이), 자연 색상
부가물
윤활제, 이형제
특별 특성
열안정성
내화학성에
General Chemical Resistance
Certifications
Food contact, Food approval 10/2011, Food approval FDA 21 CFR
응용
자동차의, 전기 및 전자
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.