Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of CELCON® M90 - POM - Celanese

Material Data Center offers the following functions for CELCON® M90:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Celcon datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 8 cm³/10min ISO 1133
온도 190 °C -
하중 2.16 kg -
성형 수축률, 평행 2.0 % ISO 294-4, 2577
성형 수축률, 수직 1.9 % ISO 294-4, 2577
용융 밀도 1200 kg/m³ -
용융 열전도율 0.155 W/(m K) -
용융 비열용량 2210 J/(kg K) -
효율적 열전도도 4.85E-8 m²/s -
이형온도 140 °C -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 2760 MPa ISO 527
항복강도 65 MPa ISO 527
항복변형률 10 % ISO 527
챠피 충격 강도 , +23°C 188 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 181 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 6 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 6 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 166 °C ISO 11357-1/-3
하중하에서의 변형온도, 1.80 MPa 101 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 158 °C ISO 75-1/-2
선형 열팽창 계수, 평행 120 E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 120 E-6/K ISO 11359-1/-2
전기적 특성단위시험규격
ISO 데이터
부피 저항 8E12 Ohm*m IEC 62631-3-1
표면 저항 >1E15 Ohm IEC 62631-3-2
기타 특성단위시험규격
물에서의 흡수성 0.75 % ISO 62와 유사
조건에서의 흡습성 0.2 % ISO 62와 유사
밀도 1410 kg/m³ ISO 1183
Processing Recommendation Injection Molding단위시험규격
Pre-drying - Temperature 80 °C -
Pre-drying - Time 3 h -
Processing humidity ≤0.35 % -
용융수지온도 182 - 199 °C -
성형온도 82 - 93 °C -
도표
응력-신율 , CELCON® M90, POM, Celanese
시컨트탄성율-신율 , CELCON® M90, POM, Celanese
응력-신율(등시) 23°C, CELCON® M90, POM, Celanese
크립탄성율-시간 23°C, CELCON® M90, POM, Celanese
곡선 크리프 23°C, CELCON® M90, POM, Celanese
응력-신율(등시) 40°C, CELCON® M90, POM, Celanese
크립탄성율-시간 40°C, CELCON® M90, POM, Celanese
곡선 크리프 40°C, CELCON® M90, POM, Celanese
특징
생산 공정
사출 성형, 필름 압출, 외형 압출, 시트 압출, 기타 압출, 중공 성형, 캘린더링
인도 유형
펠렛 (입자,알갱이)
특성
Copolymer
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧, 쨀짼쨘횓 쨔횞 횁횩쩐횙 쩐횈쨍횧쨍짰횆짬, 쨉쩔쩐챌 쨔횞 쩐횈횉횁쨍짰횆짬 짹횢쩔짧
기타 정보
사E성
Drying is generally not required because Celcon® and Hostaform® acetal copolymers are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can lead to splay (silver streaking) in molded parts. For better uniformity in molding especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 80 C (180 F) for 3hours. Desiccant hopper dryers are not required. Maximum water content = 0.35%
Standard reciprocating screw injection molding machines with a high compression screw (minimum 3:1 and preferably 4:1) and low back pressure (0.35 Mpa/50 PSI) are favored. Using a low compression screw (I.E. general purpose 2:1 compression ratio) can result in unmelted particles and poor melt homogeneity. Using a high back pressure to make up for a low compression ratio may lead to excessive shear heating and deterioration of the material.

Melt Temperature: Preferred range 182-199 C (360-390 F). Melt temperature should never exceed 230 C (450 F).

Mold Surface Temperature: Preferred range 82-93 C (180-200 F) especially with wall thickness less than 1.5 mm (0.060 in.). May require mold temperature as high as 120 C (250 F) to reproduce mold surface or to assure minimal molded in stress. Wall thickness greater than 3mm (1/8 in.) may use a cooler (65 C/150 F) mold surface temperature and wall thickness over 6mm (1/4 in.) may use a cold mold surface down to 25 C (80 F). In general, mold surface temperatures lower than 82 C (180 F) may hinder weld line formation and produce a hazy surface or a surface with flow lines, pits and other included defects that can hinder part performance.
Postprocessing conditioning and moisturizing are not required. It may be necessary to fixture large or complicated parts with varying wall thickness to prevent warpage while cooling to ambient temperature.
필름 압출
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects on the extruded film. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.35%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and melt homogeneity. The design should be approximately 35% each for feed and metering sections with the remaining 30% as the transition zone.

Melt temperature: 160-220 C (320-430 F)
Postprocessing conditioning or moisturizing is not required.
기타 압출
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying is 3 hours at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.35%
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and uniform melt homogeneity. The design should be approximately 35% each for the feed and metering sections with the remaining 30% as transition zone.

Melt temperature 180-220 C (355-430F)
Postprocessing conditioning or moisturizing are not required. For thick walled sections (>3mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm thickness
프로파일 압
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can cause surface defects on the extrusion. For better uniformity especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not required. Max. moisture content = 0.035%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio of at least 3:1 and preferably 4:1 to assure good melting and melt homogeneity. The design should be approximately 35% each for feed and metering sections with the remaining 30% as the transition zone.

Melt temperature: 180-220 C (360-430 F).
Postprocessing or moisturizing is not required. For thick walled extrusions (>3 mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)
Annealing time: 10 min/mm thickness
시트 압
Drying is generally not required because Celcon materials are not hydroscopic nor are they degraded by moisture during processing. Excessive moisture can lead to surface defects. For better uniformity in sheet extrusion especially when using regrind or material that has been stored in containers open to the atmosphere, recommended drying is 3 hours at 80 C (180 F). Desiccant hopper dryers are not required. Max. water content = 0.35%.
Standard extruders with a length to diameter ratio of at least 20:1 are recommended. The screw should be a high compression ratio (at least 3:1 and preferably 4:1) to assure good melting and uniform melt homogeneity. The screw design should be approximately 35% each for the feed and metering sections with the remaining 30% as the transition zone.

Melt temperature 180-190 C (355-375 F).
Postprocessing conditioning or moisturizing is not required. For thick walled sections (>3mm or 1/8 in.), annealing is recommended to reduce internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm wall thickness
중E성
Consult product information services.
Consult product information services.
Consult product information services.
캘린더링
Consult product information services.
Consult product information services.
Consult product information services.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.