Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of HOSTAFORM® M10AE - POM - Celanese

Material Data Center offers the following functions for HOSTAFORM® M10AE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Hostaform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 0.9 cm³/10min ISO 1133
온도 190 °C -
하중 2.16 kg -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 2800 MPa ISO 527
항복강도 65 MPa ISO 527
항복변형률 9 % ISO 527
파단시 평균신율 25 % ISO 527
챠피 충격 강도 , +23°C 220 kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 200 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 10 kJ/m² ISO 179/1eA
챠피 노치드 충격 강도, -30°C 8 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
녹는점, 10°C/min 167 °C ISO 11357-1/-3
하중하에서의 변형온도, 1.80 MPa 97 °C ISO 75-1/-2
선형 열팽창 계수, 평행 130 E-6/K ISO 11359-1/-2
전기적 특성단위시험규격
ISO 데이터
상대 유전율, 100Hz 4 - IEC 62631-2-1
상대 유전뮬, 1MHz 4 - IEC 62631-2-1
소산 인자, 100Hz 20 E-4 IEC 62631-2-1
소산 인자, 1MHz 50 E-4 IEC 62631-2-1
부피 저항 1E12 Ohm*m IEC 62631-3-1
표면 저항 1E14 Ohm IEC 62631-3-2
전기 압력 28 kV/mm IEC 60243-1
기타 특성단위시험규격
물에서의 흡수성 0.65 % ISO 62와 유사
조건에서의 흡습성 0.2 % ISO 62와 유사
밀도 1410 kg/m³ ISO 1183
도표
점도-변형률 , HOSTAFORM® M10AE, POM, Celanese
전단-변형률 , HOSTAFORM® M10AE, POM, Celanese
응력-신율 , HOSTAFORM® M10AE, POM, Celanese
시컨트탄성율-신율 , HOSTAFORM® M10AE, POM, Celanese
특징
생산 공정
사출 성형, 필름 압출, 외형 압출, 시트 압출, 기타 압출, 중공 성형
인도 유형
펠렛 (입자,알갱이)
부가물
이형제
특성
Copolymer
지역별 검색
쨘횕쩐횈쨍횧쨍짰횆짬, 짱쨌쨈, 쩐횈쩍횄쩐횈 횇횂횈챵쩐챌 횁철쩔짧, 쨀짼쨘횓 쨔횞 횁횩쩐횙 쩐횈쨍횧쨍짰횆짬, 쨉쩔쩐챌 쨔횞 쩐횈횉횁쨍짰횆짬 짹횢쩔짧
기타 정보
필름 압출
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
기타 압출
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
프로파일 압
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
시트 압
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
중E성
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with plasticating screws (20 to 25 D) will fit.

Melt temperature 180-190 °C
Mould-surface temperature 60-100 °C



Conditioning e.g. moisturizing is not necessary.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.