Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Staramide PF00AES - (PA66+PA6)-GF - Eurostar Engineering Plastics

Material Data Center offers the following functions for Staramide PF00AES:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Staramide datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
기계적 특성단위시험규격
ISO 데이터
인장탄성률 16000 MPa ISO 527
파단시 강도 210 MPa ISO 527
파단시 신율 2 % ISO 527
굴곡 계수, 23°C 15000 MPa ISO 178
Izod충격강도, +23°C 55 kJ/m² ISO 180/1U
아이조드 충격은 노치, +23°C 13 kJ/m² ISO 180/1A
아이조드 충격은 노치 11 kJ/m² ISO 180/1A
온도 -40 °C -
로크웰 경도 L 114 - ISO 2039-2
열적 특성단위시험규격
ISO 데이터
하중하에서의 변형온도, 1.80 MPa 235 °C ISO 75-1/-2
비카트 연화 온도, A 240 °C ISO 306
비카트 연화 온도, B 230 °C ISO 306
선형 열팽창 계수, 평행 12 E-6/K ISO 11359-1/-2
선형 열팽창 계수, 수직 136 E-6/K ISO 11359-1/-2
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 3.0 mm -
ASTM 데이터
UL94 난연성 HB - UL 94
테스트 두께 0.75 mm -
전기적 특성단위시험규격
ISO 데이터
상대 유전뮬, 1MHz 3.2 - IEC 62631-2-1
소산 인자, 1MHz 150 E-4 IEC 62631-2-1
부피 저항 >1E13 Ohm*m IEC 62631-3-1
표면 저항 >1E15 Ohm IEC 62631-3-2
전기 압력 19 kV/mm IEC 60243-1
CTI 500 - IEC 60112
기타 특성단위시험규격
물에서의 흡수성 2.75 % ISO 62와 유사
조건에서의 흡습성 0.85 % ISO 62와 유사
밀도 1580 kg/m³ ISO 1183
특징
생산 공정
사출 성형
지역별 검색
짱쨌쨈
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.