Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of HOSTAFORM® C 2521 G - POM - Celanese

Material Data Center offers the following functions for HOSTAFORM® C 2521 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Hostaform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Características de processamento/físicasValorUnidadeMétodo de ensaio
ISO Dados
Índice de fluidez volumétrico, MVR 1.5 cm³/10min ISO 1133
Temperatura 190 °C -
Carga 2.16 kg -
Propriedades mecânicasValorUnidadeMétodo de ensaio
ISO Dados
Módulo de tração 2100 MPa ISO 527
Tensão no escoamento 44 MPa ISO 527
Deformação no escoamento 12 % ISO 527
Deformação nominal na ruptura 15 % ISO 527
Resistência ao impacto Charpy , +23°C 50 kJ/m² ISO 179/1eU
Resistência ao impacto Charpy, -30°C 50 kJ/m² ISO 179/1eU
Res. impacto Charpy c/entalhe, +23°C 5 kJ/m² ISO 179/1eA
Res. impacto Charpy c/entalhe, -30°C 4.5 kJ/m² ISO 179/1eA
Propriedades térmicasValorUnidadeMétodo de ensaio
ISO Dados
Temperatura de fusão, 10°C/min 165 °C ISO 11357-1/-3
Temperatura de deflexão térmica, 1.80 MPa 84 °C ISO 75-1/-2
Coef. de expansão térmica linear, paralelo 100 E-6/K ISO 11359-1/-2
Propriedades elétricasValorUnidadeMétodo de ensaio
ISO Dados
Constante dielétrica, 100Hz 3.8 - IEC 62631-2-1
Constante dielétrica, 1MHz 3.8 - IEC 62631-2-1
Fator de dissipação dielétrica, 100Hz 20 E-4 IEC 62631-2-1
Fator de dissipação dielétrica, 1MHz 70 E-4 IEC 62631-2-1
Resistividade volumétrica específica 1E12 Ohm*m IEC 62631-3-1
Resistividade superficial específica 1E14 Ohm IEC 62631-3-2
Resistência elétrica 35 kV/mm IEC 60243-1
Outras propriedadesValorUnidadeMétodo de ensaio
Absorção de água 0.8 % Sim. to ISO 62
Absorção de umidade 0.2 % Sim. to ISO 62
Densidade 1340 kg/m³ ISO 1183
Recomendação de processamento Moldagem por injeçãoValorUnidadeMétodo de ensaio
Pré-secagem - temperatura 100 - 120 °C -
Pré-secagem - tempo 3 - 6 h -
Umidade do processamento ≤0.2 % -
Temperatura da massa 190 - 210 °C -
Temperatura do molde 80 - 120 °C -
Diagrama
Tensão - deformação , HOSTAFORM® C 2521 G, POM, Celanese
Módulo secante - deformação , HOSTAFORM® C 2521 G, POM, Celanese
Características
Processamento
Moldagem por injeção, Extrusão de laminas, Extrusão de perfis, Extrusão de chapas, Outros tipos de extrusão, Moldagem por sopro
Forma de entrega
Granulos
Aditivos
Lubrificantes, Desmoldante
Características
Estabilidade térmica, Copolímero
Resistência Química
Resistência do alcalóide, Resistência aos solventes, Estabilidade hidrolítica, Resistência à oxidação
Aplicaciones
Automóvel
Disponibilidade regional
América do Norte, Europa
Outras informações
Moldagem por injeção
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %
Standard injection moulding machines with three phase (15 to 25 D)
plasticating screws will fit.

Conditioning e.g. moisturizing is not necessary.
Extrusão de làminas
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
Outros tipos de extrusão
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
Extrusão de perfis
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
Extrusão de chapas
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com