Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® W2320 003 PRO TR AT - POM - BASF

Material Data Center offers the following functions for Ultraform® W2320 003 PRO TR AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informação do produto
Very free-flowing grade for injection molding with special lubricant to minimize friction,wear, stick-slip and squeaking.

Ultraform® PRO offers a comprehensive service package, which supports customers in product development for the medical technology market.

Additional compliances may also be available. Please contact your local representative or the Ultraplaste Infopoint (E-Mail: ultraplaste.infopoint@basf.com, Telefon: 49 621-60-78780, Fax: 49 621-60-78730).

For notice:
However, BASF has not designed or tested its plastics with respect to all of the special requirements related to their use in medical devices (defined in risk classes I to III according to the European and US Medical Device legislation) and pharmaceutical applications. Therefore BASF makes no warranties, express or implied, concerning the suitability of any BASF plastics for use in any medical device and pharmaceutical applications.

Abbreviated designation according to ISO 1043-1: POM
Designation according to ISO 29988-POM-K,,M-GNRS2,5-2
Características de processamento/físicasValorUnidadeMétodo de ensaio
ISO Dados
Índice de fluidez volumétrico, MVR 25 cm³/10min ISO 1133
Temperatura 190 °C -
Carga 2.16 kg -
Contração após a moldagem, paralelo 2.0 % ISO 294-4, 2577
Contração após a moldagem, perpendicular 1.9 % ISO 294-4, 2577
Propriedades mecânicasValorUnidadeMétodo de ensaio
ISO Dados
Módulo de tração 2500 MPa ISO 527
Tensão no escoamento 50 MPa ISO 527
Deformação no escoamento 5.5 % ISO 527
Deformação nominal na ruptura 37 % ISO 527
Resistência ao impacto Charpy , +23°C 110 kJ/m² ISO 179/1eU
Resistência ao impacto Charpy, -30°C 95 kJ/m² ISO 179/1eU
Res. impacto Charpy c/entalhe, +23°C 5 kJ/m² ISO 179/1eA
Res. impacto Charpy c/entalhe, -30°C 4.4 kJ/m² ISO 179/1eA
Propriedades térmicasValorUnidadeMétodo de ensaio
ISO Dados
Temperatura de fusão, 10°C/min 167 °C ISO 11357-1/-3
Temperatura de deflexão térmica, 1.80 MPa 92 °C ISO 75-1/-2
Coef. de expansão térmica linear, paralelo 125 E-6/K ISO 11359-1/-2
Propriedades elétricasValorUnidadeMétodo de ensaio
ISO Dados
Constante dielétrica, 100Hz 3.5 - IEC 62631-2-1
Constante dielétrica, 1MHz 3.5 - IEC 62631-2-1
Fator de dissipação dielétrica, 100Hz 9 E-4 IEC 62631-2-1
Fator de dissipação dielétrica, 1MHz 55 E-4 IEC 62631-2-1
Resistividade volumétrica específica 1E11 Ohm*m IEC 62631-3-1
Resistividade superficial específica 1E14 Ohm IEC 62631-3-2
Índice comparativo de linha de fuga 600 - IEC 60112
Outras propriedadesValorUnidadeMétodo de ensaio
Absorção de água 0.8 % Sim. to ISO 62
Absorção de umidade 0.2 % Sim. to ISO 62
Densidade 1380 kg/m³ ISO 1183
Diagrama
Viscosidade - taxa de cisalhamento , Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão de cisalhamento - taxa de cisalhamento , Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de cisalhamento dinâmico - temperatura , Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação , Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo secante - deformação , Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 23°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 23°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 23°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 40°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 40°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 40°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 60°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 60°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 60°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 80°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 80°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 80°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 100°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 100°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 100°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Tensão - deformação (isocrônico) 120°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de fluência - tempo 120°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Curva de fluencia 120°C, Ultraform® W2320 003 PRO TR AT, POM, BASF
Volume específico - temperatura (pvT) , Ultraform® W2320 003 PRO TR AT, POM, BASF
Módulo de tração - temperatura , Ultraform® W2320 003 PRO TR AT, POM, BASF
Características
Processamento
Moldagem por injeção
Forma de entrega
Granulos
Aditivos
Lubrificantes, Desmoldante
Características
Grau tribológico
Aplicaciones
Médico
Disponibilidade regional
Outras informações
Moldagem por injeção
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 210 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min

Processing

Usual single-flighted three-section screws with an effective screw length of at least 15 D, better 20 - 23 D are suitable for the injection molding of Ultraform.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.


Postprocessing

If parts were produced at a comparatively low mold temperature (e.g. in order to obtain short cycle times) and must not change their geometry in use thermal postprocessing inducing dimensional changes by postcrystallization may be necessary. In such cases parts should be stored in an oven with recirculated air at temperatures of 100 - 130 °C until dimensions don't change significantly any further. The time needed for this has to be determined experimentally.
Resistência em meio químico
Ácidos
Ácido Acético (5% em massa) (23°C)
Ácido Láctico (10% em massa) (23°C)
Ácido Hidroclorídrico (36% em massa) (23°C)
Ácido Nítrico (40% em massa) (23°C)
Ácido Sulfúrico (38% em massa) (23°C)
Ácido Sulfúrico (5% em massa) (23°C)
Solução de Ácido Crômico (40% em massa) (23°C)
Bases
Solução de Hidróxido de Sódio (35% em massa) (23°C)
Solução de Hidróxido de Sódio (1% em massa) (23°C)
Solução de Hidróxido de Amônio (10% em massa) (23°C)
Álcoois
Álcool isopropílico (23°C)
Metanol (23°C)
Etanol (23°C)
Hidrocarbonetos
n-Hexano (23°C)
Tolueno (23°C)
Iso-Octano (23°C)
Cetonas
Acetona (23°C)
Éteres
Di-etil éter (23°C)
Óleos Minerais
Óleo de motor multissérie SAE 10W40 (130°C)
Óleo de engrenagem hipóide SAE 80/90 (130°C)
Combustíveis Padrões
Líquido 1 ISO 1817 (60°C)
Líquido 2 ISO 1817 (60°C)
Líquido 3 ISO 1817 (60°C)
Líquido 4 ISO 1817 (60°C)
Combustível padrão sem álcool (pref. Líquico C ISO 1817) (23°C)
Combustível padrão com álcool (pref. Líquico 4 ISO 1817) (23°C)
Diesel (pref. Líquido F ISO 1817) (23°C)
Diesel (pref. Líquido F ISO 1817) (>90°C)
Soluções de sais
Solução de Cloreto de Sódio (10% em massa) (23°C)
Solução de Hipoclorito de Sódio (10% em massa) (23°C)
Solução de Carbonato de Sódio (20% em massa) (23°C)
Solução de Carbonato de Sódio (2% em massa) (23°C)
Outras
Acetato de Etila (23°C)
Peróxido de Hidrogênio (23°C)
Fluido de freio DOT No. 4 (130°C)
Etileno Glicol (50% em massa) em água (108°C)
(50% Ácido Oleico + 50% Azeite de Oliva) (23°C)
Água (23°C)
Água Deionizada (90°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.