Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Utec® 6541 - (PE-UHMW) - Braskem

Material Data Center offers the following functions for Utec® 6541:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Utec datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Propriedades mecânicasValorUnidadeMétodo de ensaio
ISO Dados
Tensão no escoamento 17 MPa ISO 527
Tensão na ruptura 30 MPa ISO 527
Deformação na ruptura 350 % ISO 527
Resistência ao impacto Charpy, +23°C 100 kJ/m² ISO 179/1eU
Dureza Shore D 64 - ISO 7619-1
ASTM Dados
Resistência à tração no escoamento 17 MPa ASTM D 638
Resistência à tração na ruptura 30 MPa ASTM D 638
Deformação na ruptura 300 % ASTM D 638
Dureza Shore D 64 - ASTM D 2240
Impacto Izod com entalhe, 1/8 in N J/m ASTM D 256
Propriedades térmicasValorUnidadeMétodo de ensaio
ISO Dados
Temperatura de amolecimento Vicat , A 128 °C ISO 306
ASTM Dados
Coeficiente de expansão térmica, long. 150 E-6/K ASTM D 696
DTUL @ 66 psi 79 °C ASTM D 648
DTUL @ 264 psi 48 °C ASTM D 648
Temperatura de fusão 133 °C ASTM D 3418
Condutividade térmica, estado sólido 0.0577 W/(m K) ASTM C 177
Propriedades elétricasValorUnidadeMétodo de ensaio
ASTM Dados
Resistência elétrica, tempo curto 90 kV/mm ASTM D 149
Resistividade superficial específica 1E12 Ohm ASTM D 257
Resistividade volumétrica específica 1E14 Ohm*cm ASTM D 257
Outras propriedadesValorUnidadeMétodo de ensaio
Absorção de água, 24hr 0.01 % ASTM D 570
Densidade 925 kg/m³ ASTM D 792
Viscosidade intrínseca 28 dl/g -
Bulk Density 450 kg/m³ -
Características
Processamento
Extrusão de perfis, Moldagem por compressão
Características especiais
Alto impacto.
Características
Grau tribológico
Certifications
Contacto com alimentos, Aprovação de alimentos FDA 21 CFR
Disponibilidade regional
América do Norte, Europa, America Centra e do Sul
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com