Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® L-GF15 - PA12-GF15 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® L-GF15:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informação do produto

Glass fibre reinforced (15%) PA12 resin for the injection moulding of rigid and tough parts


VESTAMID® L-GF15 NC is a glass fiber –reinforced heat stabilized Polyamide 12 for injection molding. The material contains about 15% glass fibers, an ageing protective agent and a processing aid for a fast and even form filling. Due to the reinforcement moldings from this compound exhibit a higher strength and good heat resistance, excellent for gear housings for electric window openers in cars.


Further advantages of VESTAMID® L-GF15 NC are the characterizing properties of PA12, e.g., low water absorption, good dimensional stability and nearly constant mechanical properties at changing ambient humidity.

  
VESTAMID® L-GF15 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

 
The use of colorants may change property values.


Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.


For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 
 

The values presented are typical or average values, they do not constitute a specification.

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM

OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM
Características de processamento/físicasSeco / CondUnidadeMétodo de ensaio
ISO Dados
Índice de fluidez volumétrico, MVR 55 / * cm³/10min ISO 1133
Temperatura 275 / * °C -
Carga 5 / * kg -
Contração após a moldagem, paralelo 0.3 / * % ISO 294-4, 2577
Contração após a moldagem, perpendicular 0.7 / * % ISO 294-4, 2577
Propriedades mecânicasSeco / CondUnidadeMétodo de ensaio
ISO Dados
Módulo de tração 4200 / 3600 MPa ISO 527
Tensão no escoamento 90 / 81 MPa ISO 527
Deformação no escoamento 4 / 4 % ISO 527
Deformação nominal na ruptura 5 / 4 % ISO 527
Resistência ao impacto Charpy , +23°C 64 / 49 kJ/m² ISO 179/1eU
Type of failure C / C - -
Resistência ao impacto Charpy, -30°C 80 / 55 kJ/m² ISO 179/1eU
Type of failure C / C - -
Res. impacto Charpy c/entalhe, +23°C 12 / 9 kJ/m² ISO 179/1eA
Type of failure C / C - -
Res. impacto Charpy c/entalhe, -30°C 11 / 7 kJ/m² ISO 179/1eA
Type of failure C / C - -
Propriedades térmicasSeco / CondUnidadeMétodo de ensaio
ISO Dados
Temperatura de fusão, 10°C/min 178 / * °C ISO 11357-1/-3
Temperatura de deflexão térmica, 1.80 MPa 160 / * °C ISO 75-1/-2
Temperatura de deflexão térmica, 0.45 MPa 175 / * °C ISO 75-1/-2
Temperatura de amolecimento Vicat, B 170 / * °C ISO 306
Coef. de expansão térmica linear, paralelo 80 / * E-6/K ISO 11359-1/-2
Flamabilidade a 1.5mm esp. nom. HB / * class IEC 60695-11-10
Espessuras do tubo de teste 1.6 / * mm -
Cartão Amarelo (yellow card) disponível sim / * - -
Cartão Amarelo (yellow card) disponível sim / * - -
Propriedades elétricasSeco / CondUnidadeMétodo de ensaio
ISO Dados
Constante dielétrica, 100Hz 4 / 5.2 - IEC 62631-2-1
Constante dielétrica, 1MHz 3.4 / 3.3 - IEC 62631-2-1
Fator de dissipação dielétrica, 100Hz 380 / - E-4 IEC 62631-2-1
Fator de dissipação dielétrica, 1MHz 260 / 450 E-4 IEC 62631-2-1
Resistividade volumétrica específica >1E13 / 1.8E12 Ohm*m IEC 62631-3-1
Resistência elétrica 50 / 47 kV/mm IEC 60243-1
Índice comparativo de linha de fuga 600 / - - IEC 60112
Outras propriedadesSeco / CondUnidadeMétodo de ensaio
Absorção de água 1.3 / * % Sim. to ISO 62
Absorção de umidade 0.6 / * % Sim. to ISO 62
Densidade 1120 / - kg/m³ ISO 1183
Produção de amostra para testeValorUnidadeMétodo de ensaio
ISO Dados
Moldagem por injeção, temperatura da massa 260 °C ISO 294
Moldagem por injeção, temperatura do molde 80 °C ISO 294
Moldagem por injeção, velocidade de injeção 200 mm/s ISO 294
Moldagem por injeção, pressão de recalque 70 MPa ISO 294
Diagrama
Viscosidade - taxa de cisalhamento , VESTAMID® L-GF15, PA12-GF15, Evonik
Tensão de cisalhamento - taxa de cisalhamento , VESTAMID® L-GF15, PA12-GF15, Evonik
Módulo de cisalhamento dinâmico - temperatura , VESTAMID® L-GF15 (dry), PA12-GF15, Evonik
Tensão - deformação , VESTAMID® L-GF15 (dry), PA12-GF15, Evonik
Módulo secante - deformação , VESTAMID® L-GF15 (dry), PA12-GF15, Evonik
Tensão - deformação (isocrônico) 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Módulo de fluência - tempo 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Curva de fluencia 23°C, VESTAMID® L-GF15 (cond.), PA12-GF15, Evonik
Módulo de tração - temperatura , VESTAMID® L-GF15 (dry), PA12-GF15, Evonik
Características
Processamento
Moldagem por injeção
Forma de entrega
Granulos, Cor natural
Aditivos
Lubrificantes
Características especiais
Estável contra o calor
Aplicaciones
Automóvel
Disponibilidade regional
América do Norte, Europa, Ásia Pacífico, America Centra e do Sul, Oriente/África
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.