Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Elastollan® B 80 A - (TPU-ARES) - BASF Polyurethanes GmbH

Material Data Center offers the following functions for Elastollan® B 80 A:
unit conversion, PDF datasheet print, comparison with other plastics, parameters for material models, CAE Interfaces

Check here, which other Elastollan datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
DESCRIPTION
Elastollan B 80 A is a polyester based TPU

SPECIAL PROPERTIES
good wear performance, good damping behavior and rebound elasticity
at good flexibility at low temperature, good tensile strength

TYPICAL APPLICATIONS
damping parts, hoses,

OTHER HINTS
predrying: 2-3h at 100-110°C
(air circulating oven) or 80-90°C (dehumidified air dryer),
max. content of humidity before processing: 0,02%
annealing: 20 h at 100°C in order to get optimum properties

CHEMICAL RESISTANCE
For detailed information on the chemical resistance of our
materials refer to this list of chemical resistance
机械性能价值单位Test Standard
ISO数据
100%应变时的应力 5 MPa ISO 527
断裂应力 TPE 50 MPa ISO 527
断裂应变 TPE >300 % ISO 527
23°C时恒定应变下的永久变形, 24h 20 % ISO 815
70°C时恒定应变下的永久变形, 24h 30 % ISO 815
撕裂强度 85 kN/m ISO 34-1
耐磨性 30 mm³ ISO 4649
肖氏硬度A 82 - ISO 7619-1
其它性能价值单位Test Standard
密度 1190 kg/m³ ISO 1183
函数
粘度-剪切速度 , Elastollan® B 80 A, (TPU-ARES), BASF PU
剪切应力-剪切速度 , Elastollan® B 80 A, (TPU-ARES), BASF PU
动态剪切模量-温度 , Elastollan® B 80 A, (TPU-ARES), BASF PU
应力-应变(TPE) , Elastollan® B 80 A, (TPU-ARES), BASF PU
典型数据
加工方法
注塑
地区供应
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.