Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of HOSTAFORM® C 9021 ECO-B - POM - Celanese

Material Data Center offers the following functions for HOSTAFORM® C 9021 ECO-B:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Hostaform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
Chemical abbreviation according to ISO 1043-1: POM Molding compound ISO 29988- POM-K, M-GNR, 03-002 POM copolymer Standard-Injection molding type with high rigidity, hardness and toughness; good chemical resistance to solvents, fuel and strong alkalis as well as good hydrolysis resistance; high resistance to thermal and oxidative degradation. Monomers and additives are listed in EU-Regulation (EU) 10/2011 FDA compliant according to 21 CFR 177.2470 .Burning rate ISO 3795 and FMVSS 302 < 75 mm/min for a thickness more than 1 mm. Ranges of applications: automotive engineering, precision engineering, electric and electronical industry, domestic appliances. FDA = Food and Drug Administration (USA) FMVSS = Federal Motor Vehicle Safety Standard (USA) UL = Underwriters Laboratories (USA).
ECO-B: Hostaform ECO-B is a POM-Copolymer with the same properties and performance as standard grades but produced with sustainability in mind. Using a mass-balance approach, biogenic feedstocks are used to offset the use of fossil-based raw materials and decrease greenhouse gas emissions. The process is audited and certified according to the ISCC Plus mass balance approach.

Flammability @1.6mm nom. thickn.HB-
Flammability at thickness h (3 mm)HBUL recognition (h)
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 8 cm³/10min ISO 1133
温度 190 °C -
载荷 2.16 kg -
模塑收缩率, 平行 2.0 % ISO 294-4, 2577
模塑收缩率, 垂直 1.9 % ISO 294-4, 2577
熔体密度 1200 kg/m³ -
熔体 0.155 W/(m K) -
熔体的比热 2210 J/(kg K) -
有效导热率a 4.85E-8 m²/s -
喷射温度 140 °C -
机械性能价值单位Test Standard
ISO数据
拉伸模量 2850 MPa ISO 527
屈服应力 64 MPa ISO 527
屈服伸长率 9 % ISO 527
名义断裂伸长率 30 % ISO 527
无缺口简支梁冲击强度, +23°C 220 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 220 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 6.5 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 6 kJ/m² ISO 179/1eA
热性能价值单位Test Standard
ISO数据
熔融温度, 10°C/min 166 °C ISO 11357-1/-3
热变形温度, 1.80 MPa 104 °C ISO 75-1/-2
热变形温度, 0.45 MPa 160 °C ISO 75-1/-2
线性热膨胀系数, 平行 110 E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 110 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 1.5 mm -
厚度为h时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 3.0 mm -
Yellow Card 现存 是的 - -
电性能价值单位Test Standard
ISO数据
相对介电常数., 100Hz 4 - IEC 62631-2-1
相对介电常数., 1MHz 4 - IEC 62631-2-1
介质损耗因子, 100Hz 20 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 50 E-4 IEC 62631-2-1
体积电阻率 1E12 Ohm*m IEC 62631-3-1
表面电阻率 1E14 Ohm IEC 62631-3-2
介电强度 35 kV/mm IEC 60243-1
其它性能价值单位Test Standard
吸水性 0.65 % 类似ISO 62
吸湿性 0.2 % 类似ISO 62
密度 1410 kg/m³ ISO 1183
函数
粘度-剪切速度 , HOSTAFORM® C 9021 ECO-B, POM, Celanese
剪切应力-剪切速度 , HOSTAFORM® C 9021 ECO-B, POM, Celanese
动态剪切模量-温度 , HOSTAFORM® C 9021 ECO-B, POM, Celanese
应力-应变.  , HOSTAFORM® C 9021 ECO-B, POM, Celanese
正割模量-应变.  , HOSTAFORM® C 9021 ECO-B, POM, Celanese
应力-应变(等时的) 23°C, HOSTAFORM® C 9021 ECO-B, POM, Celanese
蠕变模量-时间. 23°C, HOSTAFORM® C 9021 ECO-B, POM, Celanese
蠕变曲线 23°C, HOSTAFORM® C 9021 ECO-B, POM, Celanese
典型数据
加工方法
注塑, 薄膜挤出成型, 异型材挤出成型, 片材挤出成型, 其它挤出成型, 吹塑
供货形式
粒料
添加剂
脱模助剂
特征
共聚物
耐化学试剂
耐碱性, 耐溶剂性, 水解稳定
Certifications
生物相容, 可食品接触的, 10/2011认证, FDA 21 CFR认证, ISCC Plus
应用
汽车, 电子电气
地区供应
其他信息
注塑成型
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %
Standard injection moulding machines with three phase (15 to 25 D)
plasticating screws will fit.

Conditioning e.g. moisturizing is not necessary.
薄膜挤出成型
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %
Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C
Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
其E烦龀尚
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
板材挤出成型
General drying is not necessary due to low moisture absorption of
the resin.

In case of bad storage conditions (water contact or condensed water)
the use of a recirculating air dryer (100 to 120 °C / max. 40 mm
layer / 3 to 6 hours) is recommended.

Max. Water content 0,2 %

Standard extruders with grooved feed zone and short compression
screws (minimum 25 D) will fit.

Melt temperature 180-190 °C



Conditioning e.g. moisturizing is not necessary.

In case of very thick wall thickness profiles after-annealing it is
recommended to reduce internal stress.

Annealing temperature 130-140 °C
Annealing time 10 min/mm thickness
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com