Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of LUPOS SG5009 - (ASA+PMMA) - LG Chem

Material Data Center offers the following functions for LUPOS SG5009:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Lupos datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
加工/物理特性价值单位Test Standard
ISO数据
熔融指数, MFI 6.5 g/10min ISO 1133
温度 220 °C -
负载 10 kg -
模塑收缩率, 平行 0.7 % ISO 294-4, 2577
模塑收缩率, 垂直 0.7 % ISO 294-4, 2577
ASTM数据
熔融指数, MFI 6.5 g/10min ASTM D 1238
温度 220 °C -
负载 10 kg -
模压收缩率, 平行 0.007 mm/mm ASTM D 955
模压收缩率, TD 0.007 mm/mm ASTM D 955
机械性能价值单位Test Standard
ISO数据
拉伸模量 2150 MPa ISO 527
屈服应力 50 MPa ISO 527
屈服伸长率 4.3 % ISO 527
断裂应力 43 MPa ISO 527
断裂伸长率 30 % ISO 527
弯曲模量, 23°C 2000 MPa ISO 178
弯曲强度 70 MPa ISO 178
简支梁缺口冲击强度, +23°C 5.5[1] kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 1.1[1] kJ/m² ISO 179/1eA
悬臂梁缺口冲击强度, +23°C 5.4[1] kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 2.2[1] kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 - 温度 -30 °C -
洛克硬度 R 119 - ISO 2039-2
ASTM数据
拉伸模量 2284 MPa ASTM D 638
屈服应力 53 MPa ASTM D 638
断裂拉伸强度 49 MPa ASTM D 638
屈服伸长率 4.6 % ASTM D 638
断裂伸长率 30 % ASTM D 638
弯曲模量 2042 MPa ASTM D 790
弯曲强度 75.5 MPa ASTM D 790
洛克硬度 R 119 - ASTM D 785
悬臂梁缺口冲击强度, 1/8 in 54 J/m ASTM D 256
悬臂梁缺口冲击强度, 1/4 in 52 J/m ASTM D 256
低温悬臂梁缺口冲击强度, Low-Temperature 28.5 J/m ASTM D 256
温度 -30 °C -
1: 4 mm
热性能价值单位Test Standard
ISO数据
热变形温度, 1.80 MPa 75 °C ISO 75-1/-2
热变形温度, 0.45 MPa 80 °C ISO 75-1/-2
维卡软化温度, B 90 °C ISO 306
线性热膨胀系数, 平行 78 E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 91 E-6/K ISO 11359-1/-2
ASTM数据
热释放速率, 平行 78 E-6/K ASTM D 696
热释放速率, 垂直 91 E-6/K ASTM D 696
DTUL @ 66 psi 85 °C ASTM D 648
DTUL @ 264 psi 80 °C ASTM D 648
维卡温度 90 °C ASTM D 1525
电性能价值单位Test Standard
ISO数据
体积电阻率 1E15 Ohm*m IEC 62631-3-1
表面电阻率 1E15 Ohm IEC 62631-3-2
ASTM数据
电介质强度, 短时 23 kV/mm ASTM D 149
表面电阻率 1E15 Ohm ASTM D 257
体积电阻率 1E17 Ohm*cm ASTM D 257
其它性能价值单位Test Standard
吸湿性 0.2 % 类似ISO 62
密度 1150 kg/m³ ISO 1183
密度 1150 kg/m³ ASTM D 792
加工推荐(注塑)价值单位Test Standard
预干燥-温度 70 - 80 °C -
预干燥-时间 3 - 4 h -
加工湿度 ≤0.01 % -
注塑熔体温度 210 - 240 °C -
模具温度 40 - 60 °C -
1区 210 - 230 °C -
2区 210 - 230 °C -
3区 210 - 230 °C -
喷嘴温度 220 - 240 °C -
典型数据
加工方法
注塑
供货形式
黑色
特殊性能
经耐紫外线处理的/耐气候的
特征
抗划性
应用
汽车, 通用
地区供应
北美, 欧洲, 亚太, 中南美洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.