Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultraform® H2320 006 AT - POM - BASF

Material Data Center offers the following functions for Ultraform® H2320 006 AT:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultraform datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
具有较高流动性的高分子量等级, 用于相对厚壁模制品的注塑。

根据ISO 1043-1: POM的缩写名称
根据ISO 29988-POM-K,,M-GNR,1-2的名称
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 2.9 cm³/10min ISO 1133
温度 190 °C -
载荷 2.16 kg -
模塑收缩率, 平行 2.1 % ISO 294-4, 2577
模塑收缩率, 垂直 2.1 % ISO 294-4, 2577
机械性能价值单位Test Standard
ISO数据
拉伸模量 2600 MPa ISO 527
屈服应力 62 MPa ISO 527
屈服伸长率 11 % ISO 527
名义断裂伸长率 30 % ISO 527
拉伸蠕变模量, 1h 1800 MPa ISO 899-1
拉伸蠕变模量, 1000h 1300 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 270 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 260 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 6.5 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 5.5 kJ/m² ISO 179/1eA
热性能价值单位Test Standard
ISO数据
熔融温度, 10°C/min 165 °C ISO 11357-1/-3
热变形温度, 1.80 MPa 95 °C ISO 75-1/-2
热变形温度, 0.45 MPa 156 °C ISO 75-1/-2
维卡软化温度, B 150 °C ISO 306
线性热膨胀系数, 平行 120 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 1.6 mm -
Yellow Card 现存 是的 - -
厚度为h时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 0.8 mm -
Yellow Card 现存 是的 - -
燃烧性-氧指数 15 % ISO 4589-1/-2
电性能价值单位Test Standard
ISO数据
相对介电常数., 100Hz 3.8 - IEC 62631-2-1
相对介电常数., 1MHz 3.8 - IEC 62631-2-1
介质损耗因子, 100Hz 10 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 50 E-4 IEC 62631-2-1
体积电阻率 1E11 Ohm*m IEC 62631-3-1
表面电阻率 1E13 Ohm IEC 62631-3-2
介电强度 40 kV/mm IEC 60243-1
相对漏电起痕指数 600 - IEC 60112
其它性能价值单位Test Standard
吸水性 0.9 % 类似ISO 62
吸湿性 0.2 % 类似ISO 62
密度 1410 kg/m³ ISO 1183
典型数据
加工方法
注塑, 薄膜挤出成型, 异型材挤出成型, 片材挤出成型, 其它挤出成型
供货形式
粒料
添加剂
脱模助剂
特征
共聚物
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min
薄膜挤出成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Blown film, Melt temperature: 175 - 180 °C
Extrusion, Flat film, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
其E烦龀尚
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Prepreg, Melt temperature: 175 - 180 °C
Extrusion, Pipes, Melt temperature: 175 - 180 °C
Extrusion, cable sheathing, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
E尾募烦龀尚
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Profiles, Melt temperature: 175 - 180 °C

Processing

Ultraform can be processed to particular advantage using three-section screws having a total length L of 20 - 25 D and a constant pitch of about 1 D. However short-compression zone screws may also be used.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.

Postprocessing

Due to the different solidification and cooling of the melt which varies according to time and place stresses may arise, especially in the case of large wall thicknesses. These stresses can be removed by subsequent heat treatment. Tempering is essential when high demands are placed on dimensional stability. It can be carried out in air, liquid wax or oil at temperatures of 130 - 150, usually 140 - 145 °C. Lower temperatures are not effective. Duration: 10 minutes per 1 mm wall thickness.
板材挤出成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 10 min
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com