Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultrasint PA6 black - PA6 - BASF

Material Data Center offers the following functions for Ultrasint PA6 black:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Ultrasint datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 24 / * cm³/10min ISO 1133
温度 240 / * °C -
载荷 2.16 / * kg -
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 220 / * °C ISO 11357-1/-3
热变形温度, 1.80 MPa 98 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 194 / * °C ISO 75-1/-2
维卡软化温度, A 216 / * °C ISO 306
维卡软化温度, B 199 / * °C ISO 306
其它性能干 / 已调节单位Test Standard
密度 1150 / - kg/m³ ISO 1183
Bulk density 490 kg/m³ -
3D Data干 / 已调节单位Test Standard
Other Standards[S]
拉伸模量, flat 3500 / 1550 MPa ISO 527
拉伸模量, upright 3550 / 1600 MPa ISO 527
拉伸强度, flat 61 / 54 MPa ISO 527
拉伸强度, upright 47 / 43 MPa ISO 527
断裂伸长率, flat 1.9 / 51 % ISO 527
断裂伸长率, upright 1.4 / 6 % ISO 527
弯曲模量, flat 3300 / 1550 MPa ISO 178
弯曲模量, upright 3500 / 1650 MPa ISO 178
无缺口简支梁冲击强度, +23°C, flat 7.1 / 12.6 kJ/m² ISO 179/1eU
无缺口简支梁冲击强度, +23°C, upright 4.1 / 6.5 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C, flat 2.5 / 4.2 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, +23°C, upright 1.7 / 2.8 kJ/m² ISO 179/1eA
Izod冲击强度, +23°C, flat 7 / 11.5 kJ/m² ISO 180/1U
Izod冲击强度, +23°C, upright 4.5 / 6.5 kJ/m² ISO 180/1U
悬臂梁缺口冲击强度, +23°C, flat 3.7 / 5.4 kJ/m² ISO 180/1A
悬臂梁缺口冲击强度, +23°C, upright 2.6 / 2.9 kJ/m² ISO 180/1A
S: These properties are reported by the producer according standards that are different to our defaults.
典型数据
加工方法
Additive Manufacturing, 镭射烧结
供货形式
粉料, 黑色
特征
热稳定性
地区供应
欧洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com