Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® X7166 - PA12 FR(30) - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® X7166:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明

Low viscosity, self-extinguishing polyamide 12 compound, free of halogen and phosphorus

VESTAMID® X7166 NC is a heat stabilized PA 12 compound containing a non-migrating flame retardant, free of halogen and phosphorus. Tested according to UL94, VESTAMID® X7166 complies with the flammability class V-2.
 
Due to the halogen- and phosphorus-free flame retardants, VESTAMID® X7166 is especially suitable for the electronic and cable industry. It can be used for injection molding as well as for wire extrusion coating.
 
VESTAMID® X7166 is supplied as cylindrical granules, ready for processing, in moisture-proof bags.

Due to the flame retardants, the melt temperature should not exceed 260°C. We recommend melt temperatures within a range of 210°C to 230°C.

Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM

加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 108 / * cm³/10min ISO 1133
温度 250 / * °C -
载荷 2.16 / * kg -
模塑收缩率, 平行 0.7 / * % ISO 294-4, 2577
模塑收缩率, 垂直 0.8 / * % ISO 294-4, 2577
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 1890 / - MPa ISO 527
屈服应力 47 / - MPa ISO 527
屈服伸长率 5.8 / - % ISO 527
名义断裂伸长率 20 / - % ISO 527
无缺口简支梁冲击强度, +23°C 57 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
简支梁冲击强度, -30°C 80 / - kJ/m² ISO 179/1eU
Type of failure C / - - -
简支梁缺口冲击强度, +23°C 3 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
简支梁缺口冲击强度, -30°C 5 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 178 / * °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 41 / * °C ISO 11357-1/-2
热变形温度, 1.80 MPa 50 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 140 / * °C ISO 75-1/-2
维卡软化温度, B 150 / * °C ISO 306
1.5mm名义厚度时的燃烧性 V-2 / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
厚度为h时的燃烧性 V-2 / * class IEC 60695-11-10
测试用试样的厚度 0.8 / * mm -
Yellow Card 现存 是的 / * - -
燃烧性-氧指数 34 / * % ISO 4589-1/-2
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 1MHz 3.6 / - - IEC 62631-2-1
介质损耗因子, 1MHz 340 / - E-4 IEC 62631-2-1
体积电阻率 1E12 / - Ohm*m IEC 62631-3-1
介电强度 28 / - kV/mm IEC 60243-1
相对漏电起痕指数 600 / - - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 1.3 / * % 类似ISO 62
吸湿性 0.6 / * % 类似ISO 62
密度 1070 / - kg/m³ ISO 1183
函数
比容-温度(pvT) , VESTAMID® X7166, PA12 FR(30), Evonik
典型数据
加工方法
注塑, 异型材挤出成型, 电线挤出, 其它挤出成型, 表面涂层
供货形式
粒料, 自然色
特殊性能
阻燃的, 无卤, 无磷, 经热稳处理的/耐热的
应用
电子电气
地区供应
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.