Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTODUR® GF30-FR3 NC - PBT-GF30 FR(17) - Evonik Operations GmbH

Material Data Center offers the following functions for VESTODUR® GF30-FR3 NC:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明

Glass Fiber Reinforced and Flame Retardant Polybutylene Terephthalate Compound

VESTODUR® GF30-FR3 is a glass fiber-reinforced (30% glass fiber), semi-crystalline thermoplastic compound for injection molding, based on polybutylene terephthalate (PBT), with a creamy-white color.
 
Test bars made of this compound are rated V-0, according UL94 by Underwriters Laboratories Inc., self-extinguishing and non-dripping.
 
This compound is especially suitable for parts which are subjected to high mechanical and thermal loads and must have a very good flame-resistance.

The incorporated flame retardant is non-migrating and does not contain polybrominated diphenyl ethers. The additive has no corrosive effects on metal inserts or neighboring metal parts.

Therefore, the compound is suitable for components of the electrical and electronical industry. Laser marking with high contrasts is possible.
 
The compounds are supplied as cylindrical pellets in polyethylene packaging.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.


FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM 
OR VISIT OUR PRODUCT AT WWW.VESTODUR.COM

加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 12 cm³/10min ISO 1133
温度 250 °C -
载荷 2.16 kg -
模塑收缩率, 平行 0.2 % ISO 294-4, 2577
模塑收缩率, 垂直 1.5 % ISO 294-4, 2577
机械性能价值单位Test Standard
ISO数据
拉伸模量 11400 MPa ISO 527
断裂应力 130 MPa ISO 527
断裂伸长率 2.2 % ISO 527
拉伸蠕变模量, 1h 11000 MPa ISO 899-1
拉伸蠕变模量, 1000h 8000 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 55 kJ/m² ISO 179/1eU
Type of failure C - -
简支梁缺口冲击强度, +23°C 9 kJ/m² ISO 179/1eA
Type of failure C - -
肖氏硬度D 84 - ISO 7619-1
热性能价值单位Test Standard
ISO数据
熔融温度, 10°C/min 223 °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 45 °C ISO 11357-1/-2
热变形温度, 1.80 MPa 216 °C ISO 75-1/-2
热变形温度, 0.45 MPa 223 °C ISO 75-1/-2
维卡软化温度, B 213 °C ISO 306
线性热膨胀系数, 平行 50 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-0 class IEC 60695-11-10
测试用试样的厚度 1.5 mm -
厚度为h时的燃烧性 V-0 class IEC 60695-11-10
测试用试样的厚度 0.8 mm -
燃烧性-氧指数 34 % ISO 4589-1/-2
电性能价值单位Test Standard
ISO数据
相对介电常数., 100Hz 4.1 - IEC 62631-2-1
相对介电常数., 1MHz 4.4 - IEC 62631-2-1
介质损耗因子, 100Hz 30 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 150 E-4 IEC 62631-2-1
体积电阻率 >1E13 Ohm*m IEC 62631-3-1
表面电阻率 1E13 Ohm IEC 62631-3-2
相对漏电起痕指数 250 - IEC 60112
其它性能价值单位Test Standard
吸水性 0.4 % 类似ISO 62
密度 1720 kg/m³ ISO 1183
函数
动态剪切模量-温度 , VESTODUR® GF30-FR3 NC, PBT-GF30 FR(17), Evonik
比容-温度(pvT) , VESTODUR® GF30-FR3 NC, PBT-GF30 FR(17), Evonik
典型数据
加工方法
注塑
供货形式
粒料, 自然色, 白色
添加剂
脱模助剂, 阻燃剂
特殊性能
阻燃的, 经光稳处理的/耐光的, 经耐紫外线处理的/耐气候的, 经热稳处理的/耐热的
特征
可镭射打标
应用
电子电气
地区供应
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.