Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Bayblend® T88 GF-30 - (PC+SAN)-I-GF30 - Covestro Deutschland AG

Material Data Center offers the following functions for Bayblend® T88 GF-30:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Bayblend datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
  • Rubber modified (PC SAN) blend
  • 31 % glass fiber filled
  • Vicat/B 120 temperature = 134 °C
  • optimized heat ageing- and UV-stability
  • very good flow
  • tensile modulus = 10000 MPa
  • good heat resistance
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 11 cm³/10min ISO 1133
温度 260 °C -
载荷 5 kg -
机械性能价值单位Test Standard
ISO数据
拉伸模量 10000 MPa ISO 527
断裂应力 135 MPa ISO 527
断裂伸长率 2 % ISO 527
热性能价值单位Test Standard
ISO数据
热变形温度, 1.80 MPa 126 °C ISO 75-1/-2
热变形温度, 0.45 MPa 134 °C ISO 75-1/-2
维卡软化温度, B 132 °C ISO 306
线性热膨胀系数, 平行 25 E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 60 E-6/K ISO 11359-1/-2
厚度为h时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 0.8 mm -
电性能价值单位Test Standard
ISO数据
相对介电常数., 100Hz 3.6 - IEC 62631-2-1
相对介电常数., 1MHz 3.4 - IEC 62631-2-1
介质损耗因子, 100Hz 30 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 85 E-4 IEC 62631-2-1
体积电阻率 >1E13 Ohm*m IEC 62631-3-1
表面电阻率 >1E15 Ohm IEC 62631-3-2
介电强度 35 kV/mm IEC 60243-1
相对漏电起痕指数 175 - IEC 60112
其它性能价值单位Test Standard
吸水性 0.4 % 类似ISO 62
吸湿性 0.1 % 类似ISO 62
密度 1380 kg/m³ ISO 1183
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 260 °C ISO 294
注塑, 模具温度 80 °C ISO 294
注塑, 注射速度 540 mm/s ISO 294
加工推荐(注塑)价值单位Test Standard
预干燥-温度 100 - 110 °C -
预干燥-时间 2 - 4 h -
加工湿度 ≤0.02 % -
注塑熔体温度 240 - 280 °C -
模具温度 70 - 100 °C -
函数
粘度-剪切速度 , Bayblend® T88 GF-30, (PC+SAN)-I-GF30, Covestro
剪切应力-剪切速度 , Bayblend® T88 GF-30, (PC+SAN)-I-GF30, Covestro
典型数据
加工方法
注塑
供货形式
粒料
添加剂
脱模助剂
特殊性能
高冲击韧性的/经抗冲改性的, 经热稳处理的/耐热的
地区供应
其他信息
注塑成型
PREPROCESSING
Max. Water content: 0.02 %
Drying temperature: 100 - 110 °C
(depending on the grade 10°C below the Vicat VST/B120 temperature, but not higher as the recommended values).
Drying time:
Circulating air drying oven (50 % fresh air) 4-8 h
Fresh air dryer (high speed dryer) 2-4 h
Dry air dryer 2-4 h

PROCESSING
Melt temperature: 240-280 °C
Mold temperature: 70-100 °C

Use open nozzle.
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.