Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of CALIBRE™ MEGARAD™ 2081-15 - PC - Trinseo
Material Data Center offers the following functions for CALIBRE™ MEGARAD™ 2081-15:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces
Check here, which other Calibre Megarad datasheets, application examples or technical articles are available in Material Data Center
Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our
disclaimer.
加工/物理特性 | 价值 | 单位 | Test Standard |
ISO数据 |
熔融指数, MFI |
15 |
g/10min |
ISO 1133 |
温度 |
300 |
°C |
- |
负载 |
1.2 |
kg |
- |
模塑收缩率, 平行 |
0.6 |
% |
ISO 294-4, 2577 |
ASTM数据 |
熔融指数, MFI |
15 |
g/10min |
ASTM D 1238 |
温度 |
300 |
°C |
- |
负载 |
1.2 |
kg |
- |
模压收缩率, 平行 |
0.006 |
mm/mm |
ASTM D 955 |
机械性能 | 价值 | 单位 | Test Standard |
ISO数据 |
拉伸模量 |
2300 |
MPa |
ISO 527 |
屈服应力 |
62 |
MPa |
ISO 527 |
屈服伸长率 |
6 |
% |
ISO 527 |
断裂应力 |
68 |
MPa |
ISO 527 |
断裂伸长率 |
130 |
% |
ISO 527 |
弯曲模量, 23°C |
2400 |
MPa |
ISO 178 |
弯曲强度 |
97 |
MPa |
ISO 178 |
简支梁缺口冲击强度, +23°C |
25 |
kJ/m² |
ISO 179/1eA |
悬臂梁缺口冲击强度, +23°C |
75 |
kJ/m² |
ISO 180/1A |
ASTM数据 |
拉伸模量 |
2206 |
MPa |
ASTM D 638 |
屈服应力 |
62.1 |
MPa |
ASTM D 638 |
断裂拉伸强度 |
68.3 |
MPa |
ASTM D 638 |
屈服伸长率 |
6 |
% |
ASTM D 638 |
断裂伸长率 |
130 |
% |
ASTM D 638 |
弯曲模量 |
2413 |
MPa |
ASTM D 790 |
弯曲强度 |
96.5 |
MPa |
ASTM D 790 |
洛克硬度 |
R 118 |
- |
ASTM D 785 |
悬臂梁缺口冲击强度, 1/8 in |
747 |
J/m |
ASTM D 256 |
热性能 | 价值 | 单位 | Test Standard |
ISO数据 |
热变形温度, 1.80 MPa |
120 |
°C |
ISO 75-1/-2 |
维卡软化温度, B |
138 |
°C |
ISO 306 |
ASTM数据 |
热释放速率, 平行 |
68.4 |
E-6/K |
ASTM D 696 |
DTUL @ 66 psi |
139[ann.] |
°C |
ASTM D 648 |
DTUL @ 264 psi |
122 |
°C |
ASTM D 648 |
维卡温度 |
143 |
°C |
ASTM D 1525 |
电性能 | 价值 | 单位 | Test Standard |
ISO数据 |
介电强度 |
17 |
kV/mm |
IEC 60243-1 |
ASTM数据 |
电介质强度, 短时 |
16.5 |
kV/mm |
ASTM D 149 |
耗散因素, 1 MHz |
0.002 |
- |
ASTM D 150 |
电介质常数, 60 Hz |
3 |
- |
ASTM D 150 |
电介质常数, 1 MHz |
3 |
- |
ASTM D 150 |
体积电阻率 |
2E17 |
Ohm*cm |
ASTM D 257 |
光学特性 | 价值 | 单位 | Test Standard |
ASTM数据 |
雾度 |
2 |
% |
ASTM D 1003 |
光透射率 |
85 |
% |
ASTM D 1003 |
折射率 |
1.59 |
- |
ASTM D 542 |
其它性能 | 价值 | 单位 | Test Standard |
吸水性 |
0.12 |
% |
类似ISO 62 |
吸湿性 |
0.15 |
% |
类似ISO 62 |
密度 |
1200 |
kg/m³ |
ISO 1183 |
吸水率, 24小时 |
0.15 |
% |
ASTM D 570 |
密度 |
1200 |
kg/m³ |
ASTM D 792 |
加工推荐(注塑) | 价值 | 单位 | Test Standard |
预干燥-温度 |
120 |
°C |
- |
预干燥-时间 |
4 |
h |
- |
注塑熔体温度 |
275 - 295 |
°C |
- |
模具温度 |
70 - 90 |
°C |
- |
典型数据
加工方法
注塑
添加剂
脱模助剂
特殊性能
透明., 消毒, Gamma irradiation sterilization, Electron beam (e-beam) sterilization
耐化学试剂
抗辐射性
Certifications
医用级, Biocompatibility ISO 10993
应用
药物
地区供应
北美, 欧洲, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com