Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Eastar™ EN001 - Copolyester - Eastman Chemical Co.

Material Data Center offers the following functions for Eastar™ EN001:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Eastar datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明

Eastar™ EN001 Copolyester is a thermoplastic polyester copolymer and is suitable for food packaging applications.

Eastar™ EN001 Copolyester has a relatively slow crystallization rate. This broadens the operating window for extrusion and forming processes and helps maintain good clarity when processing much thicker sheet. Eastar™ EN001 copolyester can also be used for injection molding applications. It is the preferred general-purpose crystallizable PET for thermoforming.

Eastar™ EN001 copolyester is regulated for use in food packaging applications in accordance with US FDA Regulation 21 CFR 177.1315. It is lawful for use under US Department of Agriculture Food Safety Inspection Service regulations as a packaging material for meat or poultry food products prepared under federal inspection.




机械性能价值单位Test Standard
ISO数据
拉伸模量 2400 MPa ISO 527
屈服应力 57 MPa ISO 527
断裂应力 25 MPa ISO 527
断裂伸长率 120 % ISO 527
弯曲模量, 23°C 2300 MPa ISO 178
Izod冲击强度, +23°C N kJ/m² ISO 180/1U
悬臂梁缺口冲击强度, +23°C 4.5 kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 3.1 kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 - 温度 -40 °C -
冲孔功, +23°C 15 J ISO 6603-2
洛克硬度 R 114 - ISO 2039-2
ASTM数据
拉伸模量 2400 MPa ASTM D 638
屈服应力 58 MPa ASTM D 638
断裂拉伸强度 25 MPa ASTM D 638
断裂伸长率 120 % ASTM D 638
弯曲模量 2500 MPa ASTM D 790
洛克硬度 112 - ASTM D 785
悬臂梁缺口冲击强度, 1/8 in 40 J/m ASTM D 256
低温悬臂梁缺口冲击强度, Low-Temperature 27 J/m ASTM D 256
温度 -40 °C -
Izod冲击强度, 1/8 in N J/m ASTM D 256
热性能价值单位Test Standard
ISO数据
热变形温度, 1.80 MPa 65 °C ISO 75-1/-2
热变形温度, 0.45 MPa 69 °C ISO 75-1/-2
ASTM数据
DTUL @ 66 psi 68.9 °C ASTM D 648
DTUL @ 264 psi 65 °C ASTM D 648
光学特性价值单位Test Standard
ASTM数据
雾度 1 % ASTM D 1003
光透射率 84 % ASTM D 1003
其它性能价值单位Test Standard
密度 1330 kg/m³ ISO 1183
密度 1330 kg/m³ ASTM D 792
典型数据
加工方法
注塑, 其它挤出成型, 热成型
特征
共聚物
Certifications
可食品接触的, FDA 21 CFR认证
应用
汽车, 包装, 运动器械
地区供应
北美, 欧洲, 亚太, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.