Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Novodur® HD M203FC - ABS - INEOS Styrolution

Material Data Center offers the following functions for Novodur® HD M203FC:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Novodur datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
Novodur® HD M203FC acrylonitrile butadiene styrene (ABS) polymer features high surface quality and good impact strength. Novodur® HD M203FC is an injection molding grade with high flowability and well balanced properties. Medical and food contact statements are available upon request.
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 31 cm³/10min ISO 1133
温度 220 °C -
载荷 10 kg -
熔体密度 927 kg/m³ -
熔体 0.218 W/(m K) -
熔体的比热 2900 J/(kg K) -
喷射温度 90 °C -
机械性能价值单位Test Standard
ISO数据
拉伸模量 2400 MPa ISO 527
屈服应力 46 MPa ISO 527
屈服伸长率 2.6 % ISO 527
名义断裂伸长率 17 % ISO 527
无缺口简支梁冲击强度, +23°C 110 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 90 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 16 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 7 kJ/m² ISO 179/1eA
热性能价值单位Test Standard
ISO数据
热变形温度, 1.80 MPa 94 °C ISO 75-1/-2
热变形温度, 0.45 MPa 98 °C ISO 75-1/-2
维卡软化温度, B 99 °C ISO 306
线性热膨胀系数, 平行 90 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 1.5 mm -
Yellow Card 现存 是的 - -
厚度为h时的燃烧性 HB class IEC 60695-11-10
测试用试样的厚度 3.0 mm -
Yellow Card 现存 是的 - -
电性能价值单位Test Standard
ISO数据
介电强度 35 kV/mm IEC 60243-1
相对漏电起痕指数 600 - IEC 60112
其它性能价值单位Test Standard
吸水性 0.95 % 类似ISO 62
密度 1050 kg/m³ ISO 1183
函数
粘度-剪切速度 , Novodur® HD M203FC, ABS, INEOS Styrolution
剪切应力-剪切速度 , Novodur® HD M203FC, ABS, INEOS Styrolution
应力-应变.  , Novodur® HD M203FC, ABS, INEOS Styrolution
正割模量-应变.  , Novodur® HD M203FC, ABS, INEOS Styrolution
典型数据
加工方法
注塑
供货形式
粒料
特殊性能
消毒, 环氧乙烷灭菌(EtO), Gamma irradiation sterilization
耐化学试剂
抗辐射性
Certifications
可食品接触的, 10/2011认证, FDA 21 CFR认证, 医用级, Biocompatibility ISO 10993, US药物六级认证, Drug Master File, Long term supply assurance
应用
药物
地区供应
北美, 欧洲, 亚太, 中南美洲, 中东/非洲
其他信息
注塑成型
PREPROCESSING

Pre-drying, Temperature: 80°C

Pre-drying, Time: 2 - 4h

PROCESSING

Melt temperature, range: 230 - 260°C

Mold temperature, range: 60 - 80°C

权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.