Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Panlite® LV-2250Z - PC - Teijin Chemicals Ltd.

Material Data Center offers the following functions for Panlite® LV-2250Z:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Panlite datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 8 cm³/10min ISO 1133
温度 300 °C -
载荷 1.2 kg -
ASTM数据
模压收缩率, 平行 0.006 mm/mm ASTM D 955
模压收缩率, TD 0.006 mm/mm ASTM D 955
机械性能价值单位Test Standard
ISO数据
拉伸模量 2400 MPa ISO 527
屈服应力 61 MPa ISO 527
屈服伸长率 6 % ISO 527
名义断裂伸长率 >50 % ISO 527
弯曲模量, 23°C 2350 MPa ISO 178
弯曲强度 93 MPa ISO 178
简支梁冲击强度, +23°C N kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 76 kJ/m² ISO 179/1eA
ASTM数据
拉伸模量 2120 MPa ASTM D 638
屈服应力 62 MPa ASTM D 638
断裂拉伸强度 80 MPa ASTM D 638
屈服伸长率 6 % ASTM D 638
断裂伸长率 140 % ASTM D 638
压缩强度 76 MPa ASTM D 695
弯曲模量 2230 MPa ASTM D 790
弯曲强度 92 MPa ASTM D 790
洛克硬度 M 77 - ASTM D 785
悬臂梁缺口冲击强度, 1/8 in 880 J/m ASTM D 256
悬臂梁缺口冲击强度, 1/4 in 140 J/m ASTM D 256
热性能价值单位Test Standard
ISO数据
热变形温度, 1.80 MPa 129 °C ISO 75-1/-2
热变形温度, 0.45 MPa 142 °C ISO 75-1/-2
维卡软化温度, B 149 °C ISO 306
线性热膨胀系数, 平行 70 E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 70 E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-2 class IEC 60695-11-10
测试用试样的厚度 1.5 mm -
厚度为h时的燃烧性 V-2 class IEC 60695-11-10
测试用试样的厚度 0.4 mm -
灼热丝燃烧指数 (GWFI) 825 °C IEC 60695-2-12
GWFI - 测试用试样厚度 1.5 mm -
灼热丝燃烧指数 (GWFI) 960 °C IEC 60695-2-12
GWFI - 测试用试样厚度 3 mm -
灼热丝引燃温度 (GWIT) 850 °C IEC 60695-2-13
GWIT - 测试用试样厚度 1.5 mm -
灼热丝引燃温度 (GWIT) 875 °C IEC 60695-2-13
GWIT - 测试用试样厚度 3 mm -
ASTM数据
UL94 燃烧性 V-2 - UL 94
测试厚度 3 mm -
热释放速率, 平行 70 E-6/K ASTM D 696
热释放速率, 垂直 70 E-6/K ASTM D 696
电性能价值单位Test Standard
ISO数据
相对介电常数, 100Hz 3.1 - IEC 62631-2-1
相对介电常数, 1MHz 3 - IEC 62631-2-1
介质损耗因子, 100Hz 10 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 90 E-4 IEC 62631-2-1
体积电阻率 >1E13 Ohm*m IEC 62631-3-1
表面电阻率 >1E15 Ohm IEC 62631-3-2
介电强度 30 kV/mm IEC 60243-1
相对漏电起痕指数 225 - IEC 60112
ASTM数据
电介质强度, 短时 30 kV/mm ASTM D 149
耗散因素, 60 Hz 0.0004 - ASTM D 150
耗散因素, 1 MHz 0.009 - ASTM D 150
电介质常数, 60 Hz 2.95 - ASTM D 150
电介质常数, 1 MHz 2.9 - ASTM D 150
体积电阻率 3E16 Ohm*cm ASTM D 257
耐电弧性 100 s ASTM D 495
光学特性价值单位Test Standard
ASTM数据
光透射率 88 % ASTM D 1003
折射率 1.58 - ASTM D 542
其它性能价值单位Test Standard
密度 1200 kg/m³ ISO 1183
吸水率, 平衡 0.2 % ASTM D 570
加工推荐(注塑)价值单位Test Standard
预干燥-温度 120 °C -
预干燥-时间 >5 h -
注塑熔体温度 270 - 320 °C -
模具温度 80 - 120 °C -
典型数据
加工方法
注塑
供货形式
粒料
添加剂
脱模助剂
特殊性能
经耐紫外线处理的/耐气候的, 透明.
应用
通用
地区供应
北美, 欧洲, 亚太, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com