Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Styroflex® 4G80 - SB - INEOS Styrolution

Material Data Center offers the following functions for Styroflex® 4G80:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Styroflex datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 18 cm³/10min ISO 1133
温度 200 °C -
载荷 5 kg -
ASTM数据
熔融指数, MFI 76 g/10min ASTM D 1238
温度 220 °C -
负载 10 kg -
模压收缩率, 平行 0.006 mm/mm ASTM D 955
机械性能价值单位Test Standard
ISO数据
拉伸模量 50 MPa ISO 527
断裂伸长率 500 % ISO 527
简支梁缺口冲击强度, +23°C 80 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 80 kJ/m² ISO 179/1eA
肖氏硬度A 80 - ISO 7619-1
肖氏硬度D 28 - ISO 7619-1
ASTM数据
拉伸模量 68.95 MPa ASTM D 638
屈服应力 2.41 MPa ASTM D 638
断裂伸长率 500 % ASTM D 638
邵氏硬度A 80 - ASTM D 2240
邵氏硬度D 28 - ASTM D 2240
悬臂梁缺口冲击强度, 1/8 in 747 J/m ASTM D 256
热性能价值单位Test Standard
ISO数据
维卡软化温度, A 38 °C ISO 306
ASTM数据
维卡温度 39.4 °C ASTM D 1525
光学特性价值单位Test Standard
ASTM数据
雾度 18 % ASTM D 1003
光透射率 81 % ASTM D 1003
折射率 1.56 - ASTM D 542
其它性能价值单位Test Standard
吸水性 0.07 % 类似ISO 62
吸湿性 0.07 % 类似ISO 62
密度 980 kg/m³ ISO 1183
密度 980 kg/m³ ASTM D 792
加工推荐(挤出)价值单位Test Standard
注塑熔体温度 170 - 240 °C -
模具温度 29.4 - 43.3 °C -
典型数据
加工方法
其它挤出成型
供货形式
粒料
特殊性能
透明.
特征
软质, 共聚物
应用
药物, 运动器械
地区供应
北美, 欧洲, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.