Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAKEEP® DC 4470 G - PEEK - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAKEEP® DC 4470 G:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Vestakeep datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
Gingiva-colored polyether ether ketone for dental applications

VESTAKEEP® DC4470 G is a gingiva-colored, high viscosity polyether ether ketone (PEEK) resin that is especially designed for removable dentures to meet the aesthetic demands of the patient.

Biocompatibility of VESTAKEEP® Dental
For VESTAKEEP® DC4470 G, biocompatibility has been tested according to ISO 10993-1 recommendations for permanent mucous membrane contact. The compound composition is optimised for high biocompatibility and superior mechanical, thermal and chemical resistance.
 
Biocompatibility test reports available for VESTAKEEP® DC4470 G
Standard Description
ISO 10993-03 Genotoxicity: Salmonella Typhimurium Reverse Mutation Test (Ames Test)
ISO 10993-05 Cytotoxicity: Quantitative Growth Inhibition Test
ISO 10993-10 Irritation: Intracutaneous Reactivity
ISO 10993-10 Sensitization: Local Lymph Node Assay
ISO 10993-11 Acute Systemic Toxicity
ISO 10993-11 Subacute / Subchronic Toxicity 14 days
ISO 10993-18 Extraction Tests
USP Class VI Acute Systemic Toxicity Intracutaneous Reactivity Muscle Implantation

Processing of VESTAKEEP® Dental
VESTAKEEP® DC4470 G can be processed by common melt processing techniques like injection molding and extrusion.
For injection molding, we recommend a melt temperature in the 380°C to 400°C range. The mold temperature should be within 160°C to 200°C, preferably 180°C.

Delivery of VESTAKEEP® Dental
VESTAKEEP® DC4470 G is supplied as granules in 25 kg boxes with moisture-proof polyethylene liners.

The values presented are typical or average values, they do not constitute a specification. 
 
FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.EVONIK.COM/MEDICAL-TECHNOLOGY
加工/物理特性价值单位Test Standard
ISO数据
熔体体积流动速度, MVR 11 cm³/10min ISO 1133
温度 380 °C -
载荷 5 kg -
机械性能价值单位Test Standard
ISO数据
拉伸模量 3600 MPa ISO 527
屈服应力 95 MPa ISO 527
屈服伸长率 5 % ISO 527
无缺口简支梁冲击强度, +23°C N kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 7.5 kJ/m² ISO 179/1eA
Type of failure C - -
热性能价值单位Test Standard
ISO数据
熔融温度, 10°C/min 340 °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 153 °C ISO 11357-1/-2
热变形温度, 1.80 MPa 155 °C ISO 75-1/-2
热变形温度, 0.45 MPa 210 °C ISO 75-1/-2
维卡软化温度, B 305 °C ISO 306
线性热膨胀系数, 平行 45 E-6/K ISO 11359-1/-2
其它性能价值单位Test Standard
吸水性 0.4 % 类似ISO 62
密度 1360 kg/m³ ISO 1183
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 400 °C ISO 294
注塑, 模具温度 180 °C ISO 294
注塑, 注射速度 200 mm/s ISO 294
典型数据
加工方法
注塑, 其它挤出成型
供货形式
粒料
特征
热稳定性
耐化学试剂
通用耐化学性
Certifications
医用级, Biocompatibility ISO 10993, US药物六级认证
应用
药物
地区供应
北美, 欧洲, 亚太, 中南美洲, 中东/非洲
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.